Phase Diagrams

Learn to read binary phase diagrams, the maps engineers use to tell which phases an alloy contains at a given temperature and composition. Find phase compositions with tie lines and phase amounts with the lever rule, follow how microstructures form as copper–nickel, lead–tin and iron–carbon alloys cool slowly, and use the iron–iron carbide diagram to explain the pearlite, ferrite and cementite in steels and cast irons.

BeginnerLesson 6 of 9 in Materials Science and Engineering Course

What you will learn

  1. Use the basic vocabulary of phase diagrams (component, phase, solid solution, solubility limit, microstructure, equilibrium) and read what a phase diagram shows and what it does not.
    • Define components, phases and solubility limits
      Tell components, phases, grains and microconstituents apart, express alloy composition in weight and atom percent, and explain what a solubility limit is.
    • Read a phase diagram as a map of equilibrium
      Explain equilibrium and metastable states, read one-component and binary phase diagrams, and use the Gibbs phase rule to explain why diagrams have the shapes they do.
  2. Read diagrams of alloys whose components dissolve completely in each other, find the compositions and amounts of the phases with tie lines and the lever rule, and explain the microstructures and properties that result from cooling.
    • Identify the phases in an isomorphous system
      Explain why some pairs of metals are completely soluble in each other and name the phases present at any point of an isomorphous diagram such as copper–nickel.
    • Find phase compositions and amounts with the lever rule
      Draw a tie line to find the composition of each phase in a two-phase field, then use the lever rule to calculate the mass fraction of each phase and convert it to a volume fraction when needed.
    • Follow microstructure and properties as isomorphous alloys cool
      Describe how compositions and amounts of phases change during slow equilibrium cooling, explain coring after faster cooling and how to remove it, and relate composition to strength and ductility.
  3. Read binary diagrams with limited solid solubility, predict the microstructures that eutectic-system alloys develop, and recognize intermediate phases and the eutectoid and peritectic reactions.
    • Read a binary eutectic diagram
      Identify the phases, solvus lines, eutectic point and eutectic isotherm of a diagram such as lead–tin, and write the eutectic reaction.
    • Predict the microstructures of eutectic-system alloys
      Follow alloys of different compositions as they cool slowly, describe the microstructure each one develops, and use the lever rule for both phases and microconstituents.
    • Recognize intermediate phases and other invariant reactions
      Distinguish terminal and intermediate solid solutions and intermetallic compounds, identify eutectoid and peritectic reactions on a diagram, and tell congruent from incongruent transformations.
  4. Read the iron–iron carbide diagram, explain how pearlite and the proeutectoid constituents form in slowly cooled steels, calculate the amounts of phases and microconstituents, and recognize the diagram's limits.
    • Read the iron–iron carbide diagram
      Name the phases of iron and steel, their crystal structures and carbon solubilities, locate the eutectic, eutectoid and peritectic points, and classify iron–carbon alloys.
    • Explain pearlite and hypoeutectoid steels
      Describe how pearlite forms from austenite, calculate its ferrite and cementite content, and find the amounts of proeutectoid ferrite and pearlite in a slowly cooled hypoeutectoid steel.
    • Analyze hypereutectoid steels, cast irons and the diagram's limits
      Find the amounts of proeutectoid cementite and pearlite in hypereutectoid steels, follow a cast iron through the eutectic, and explain how alloying and cooling rate limit what the diagram predicts.

Phase Diagrams study guide

4 chapters

1

Describe phases, solubility and equilibrium

Phases describe uniform regions of matter, while components describe their chemical ingredients. That distinction makes it possible to read a phase diagram without confusing grains, compositions and amounts. Start with solid solutions and solubility, then use temperature, pressure and composition to locate equilibrium states. The phase rule explains why some states occupy fields and others lie on fixed-temperature reaction lines.

1.1 Define components, phases and solubility limits

A copper–nickel alloy can contain two chemical ingredients and still be one phase. To describe it clearly, separate what the material is made from, what uniform regions exist, and how those regions are arranged.

Components, phases and grains

A component is a chemically distinct substance used to specify the system. Copper and nickel are the two components of a Cu–Ni alloy. The word system can name one sample or the entire family of alloys made from those components.

A phase is a homogeneous region with uniform physical and chemical characteristics. A liquid solution is one phase even though it contains both elements. Ice and liquid water are two phases of one component. BCC iron and FCC iron are also different phases: crystal structure matters as well as composition.

A grain is a crystal region with a particular orientation. A solid metal may have thousands of grains of the same phase. Grain boundaries divide orientations; they do not necessarily divide phases.

Dissolving atoms and reaching a limit

In a solid solution, atoms of a solute fit into a host crystal. Substitutional atoms replace host atoms; interstitial atoms occupy gaps. The host structure remains, so the solution is one phase. Greek letters such as α and γ identify solid phases; L identifies liquid.

The solubility limit is the greatest solute concentration a solvent can hold at a particular temperature. Beyond it, an additional phase appears. At 20 °C, about 204 g of sugar dissolves in 100 g of water. The saturated solution therefore contains

100204204+100≈67 wt% sugar.

The denominator is the mass of the whole solution. Dividing by the water mass alone gives grams per 100 g of water, a different quantity. A 75 wt% sugar mixture at this temperature contains saturated syrup and undissolved sugar. Heating raises sugar's solubility limit, so some of the solid can dissolve.

Weight percent and atom percent

Weight percent is a mass share. Atom percent is a share of the number of atoms. Equal masses of different elements generally contain different numbers of atoms because their atomic masses differ.

For 35 wt% Ni and 65 wt% Cu, choose a 100 g basis. Convert each mass to moles using atomic masses in g/mol:

nNi=35/58.69=0.596,nCu=65/63.55=1.023.

Then divide nickel moles by total moles:

1000.5960.596+1.023≈36.8 at% Ni.

A composition of 35 wt% Ni therefore does not mean 35 at% Ni. Read the axis label before doing a calculation, and keep one composition basis throughout it.

What a microscope adds

Microstructure describes the phases, their amounts, and their size, shape and arrangement in a polished, etched sample. A microconstituent is a recognizable part of that structure. Pearlite, for example, is one microconstituent containing alternating ferrite and cementite phases.

Two samples can have the same overall composition but different arrangements of phases and different mechanical behavior. Naming the components alone cannot describe that difference. Naming the phases still leaves their arrangement to be described.

Key Takeaways

  • A component names a chemical ingredient; a phase names a uniform physical and chemical region.
  • A polycrystalline solid can have many grains of one phase.
  • A solid solution retains the host crystal structure and counts as one phase.
  • Solubility limits depend on temperature; excess solute forms an additional phase.
  • Weight percent uses mass, while atom percent uses numbers of atoms.
  • A microconstituent can contain more than one phase.

1.2 Read a phase diagram as a map of equilibrium

A phase diagram is a map of equilibrium states. Its regions answer which phases can coexist at specified conditions. Reading it begins with the axes, because a water diagram and an alloy diagram vary different quantities.

What equilibrium means

At equilibrium, a system has the lowest free energy available at its temperature, pressure and composition. The phases, their compositions and their amounts stay constant. A metastable state persists even though a lower-energy state exists, because the change is very slow.

An equilibrium map has no time axis. It identifies the states approached when atoms have enough time to rearrange. Rapid cooling can preserve a different structure, so an equilibrium reading alone cannot specify a quenched product.

One component: water

A unary water diagram plots pressure against temperature. Its ice, liquid and vapor regions meet along lines of two-phase coexistence. At 1 atm, heating crosses the melting boundary at 0 °C and the boiling boundary at 100 °C.

The three boundaries meet at the triple point, about 0.01 °C and 611.657 Pa. Ice, water and vapor coexist there. Below this pressure, heating ice at constant pressure takes it directly into vapor by sublimation; there is no intervening stable liquid field.

Two components: alloys

A binary alloy diagram usually plots temperature vertically and composition horizontally at fixed pressure, commonly 1 atm or 101.325 kPa. If the axis reads wt% B, the left end is pure A and the right end is pure B.

Locate the overall composition C0 and move vertically to the temperature. A point in α means all α: its composition is C0 and its mass fraction is 1. A point in α + L means two phases coexist. The plus sign names two phases, not a new combined phase.

BoundaryWhat it separates
LiquidusAll liquid from liquid plus solid
SolidusAll solid from solid plus liquid
SolvusOne solid solution from two solid phases

Inside a two-phase field, a horizontal tie line reaches the compositions of the coexisting phases. The alloy's overall composition lies between those endpoints. Its position controls the amounts, not a third phase composition.

Why fields and horizontal lines differ

The Gibbs phase rule counts independent intensive variables. In general,

P+F=C+N,

where P is the number of phases, C the number of components, and N the number of noncompositional variables allowed to vary. For a binary diagram at fixed pressure, only temperature remains in N, so

F=3−P.

With one phase, two variables remain independent: temperature and composition can vary. With two phases, one remains: choosing temperature fixes both phase compositions. Overall composition can still change the relative amounts along that tie line; phase amounts are not counted in F.

With three phases, F=0. Temperature and all three phase compositions are fixed. This invariant equilibrium appears as a horizontal reaction line. It is the reason eutectic alloys transform at a fixed temperature, even though their phase amounts can change as the reaction proceeds.

Key Takeaways

  • Locate temperature and overall composition before naming the phase field.
  • In a single-phase field, the phase composition equals the overall composition.
  • Tie-line endpoints give the two phase compositions at one temperature.
  • For binary systems at constant pressure, the phase rule is F=3−P.
  • Equilibrium diagrams specify states, not transformation times.
2

Analyze binary isomorphous alloys

Copper and nickel form a single solid solution at every composition, making their diagram a useful starting point for alloy calculations. Read the liquidus and solidus, use a horizontal tie line to find phase compositions, and derive the phase amounts from mass balance. Following the same alloy through cooling then connects the equilibrium map to diffusion, coring and the mechanical effects of mixing atoms.

2.1 Identify the phases in an isomorphous system

An isomorphous system has complete mutual solubility in both liquid and solid. Copper and nickel illustrate how a two-component alloy can remain one solid solution across the whole composition range.

Why copper and nickel mix

The Hume–Rothery rules describe the atomic features associated with extensive substitutional solubility: atomic radii differing by less than about 15%, the same crystal structure, similar electronegativities and similar valences. They are empirical guidelines for judging compatibility.

Copper and nickel are both FCC. Their atomic radii are about 0.128 and 0.125 nm, a difference of roughly 2%. Their electronegativities, about 1.9 and 1.8, are close. Nickel can occupy copper sites without requiring a new crystal structure. Silver–gold and Al₂O₃–Cr₂O₃ are other isomorphous examples.

The solid solution is called α. A 10 wt% Ni solid and a 90 wt% Ni solid are both α; the label names the phase, not one fixed chemical formula. This differs from a compound such as Fe₃C, whose formula fixes its composition closely.

The three fields

The Cu–Ni diagram contains L at high temperature, α at low temperature, and α + L between them. The liquidus forms the upper edge of the lens-shaped two-phase field, and the solidus forms its lower edge.

At either pure-metal end, the lines meet: copper melts at 1085 °C and nickel at 1455 °C. Between those ends, an alloy generally has different liquidus and solidus temperatures. A 35 wt% Ni alloy starts freezing at about 1260 °C and finishes at about 1220 °C under equilibrium conditions.

Position of the alloy pointPhases presentComposition information
Above its liquidusLLiquid has the overall composition
Between liquidus and solidusα + LEach phase has a tie-line endpoint composition
Below its solidusαSolid has the overall composition
Read three locations

At 1100 °C and 60 wt% Ni, the point lies in α. Every part is solid α, containing 60 wt% Ni. The number of grains does not change this phase count.

At 1250 °C and 35 wt% Ni, the point lies in α + L. Solid and liquid coexist, but the label alone gives neither their compositions nor their amounts. A tie line supplies the next information.

At 1300 °C and 20 wt% Ni, the point lies above the liquidus. It is all liquid at 20 wt% Ni. A two-phase calculation would add work without describing any real second phase.

Follow an alloy vertically

For a closed alloy cooled without changing its total composition, draw a vertical path at C0. Crossing the liquidus marks the first solid; crossing the solidus marks the disappearance of the last liquid. On reheating, the solidus marks the first melting and the liquidus the end of melting.

The melting interval belongs to that alloy composition. Nickel's 1455 °C melting point is the endpoint of the entire diagram, not the solidus temperature of every nickel-containing alloy.

Key Takeaways

  • An isomorphous system has one solid-solution phase across its composition range.
  • Cu–Ni has the fields L, α + L and α, separated by the liquidus and solidus.
  • An isomorphous alloy freezes over a temperature range; a pure component freezes at one temperature.
  • A vertical cooling path keeps the overall composition fixed.

2.2 Find phase compositions and amounts with the lever rule

A tie line answers two different questions: what is each phase made of, and how much of each phase is present? Keep these questions separate. Endpoint compositions come first; phase fractions follow from mass balance.

Read compositions at the endpoints

For 35 wt% Ni at 1250 °C, draw a horizontal line across α + L. It meets the liquidus at CL=31.5 wt% Ni and the solidus at Cα=42.5 wt% Ni. These are compositions within the phases. The overall value C0=35 wt% Ni remains the composition of the entire alloy.

At this temperature, another alloy inside the same field has the same endpoints. A 38 wt% Ni alloy changes the amounts of α and L, not their compositions.

Derive the lever rule

Let Wα and WL be mass fractions. All the alloy mass and all the nickel must be accounted for:

Wα+WL=1,WαCα+WLCL=C0.

Substitute WL=1−Wα and collect terms. This gives

Wα=C0−CLCα−CL,WL=Cα−C0Cα−CL.

Each fraction uses the opposite arm: the distance from the alloy composition to the other phase's endpoint, divided by the full tie-line length.

Work the numbers and check them

The full length is 42.5−31.5=11 composition percentage points. Therefore,

Wα=35−31.511=0.318,WL=42.5−3511=0.682.

A 2.0 kg casting contains about 0.636 kg α and 1.364 kg liquid. Its nickel mass is

0.636(0.425)+1.364(0.315)≈0.700 kg,

which agrees with 35% of 2.0 kg. Fractions add to 1, and the phase closer in composition to the alloy is more abundant. Here 35 is closer to 31.5 than to 42.5, so liquid must be the larger share.

For 38 wt% Ni at the same temperature, Wα=(38−31.5)/11≈0.59. The endpoint values stayed fixed while the solid share increased.

Convert mass share to volume share

A wt% diagram gives mass fractions, not volume fractions. The volume occupied by a given mass depends on density. For two solid phases,

Vα=Wα/ραWα/ρα+Wβ/ρβ.

At 150 °C, a 40 wt% Sn alloy has α of about 11 wt% Sn and β of about 98 wt% Sn. Thus Wα=58/87≈0.667. With densities 10.7 and 7.3 g/cm³, a 1 g basis gives about 0.0623 cm³ α and 0.0457 cm³ β. Dividing by their combined volume gives Vα≈0.58. The denser α occupies a smaller volume share than mass share.

Before calculating, check that the alloy point is actually inside a two-phase field. In a single-phase field the fraction is already 1. Keep every composition on the same wt% or at% basis, and round only after computing the fractions.

Key Takeaways

  • A horizontal tie line gives phase compositions at its boundary intersections.
  • The lever rule follows from total-mass and component-mass balances.
  • Use the opposite arm divided by the total tie-line length for each mass fraction.
  • At fixed temperature, changing overall composition changes amounts within a two-phase field.
  • Divide mass fractions by densities and normalize to obtain volume fractions.
  • Check that fractions sum to 1 and reproduce the overall composition.

2.3 Follow microstructure and properties as isomorphous alloys cool

The first solid in a freezing alloy does not usually have the overall composition. As cooling continues, both phases change composition. Whether the existing solid can keep adjusting depends on diffusion.

Follow equilibrium solidification

Start with a 35 wt% Ni–65 wt% Cu liquid at 1300 °C. Its composition stays at 35 wt% Ni until the liquidus is reached near 1260 °C. The first small amount of α contains about 46 wt% Ni. It is enriched in nickel, but it is a Cu–Ni solution, not pure nickel.

As temperature falls, the liquid endpoint follows the liquidus and the solid endpoint follows the solidus. Both move toward lower nickel content. The solid amount grows while the liquid amount shrinks. At 1250 °C, the liquid contains 31.5 wt% Ni, α contains 42.5 wt% Ni, and about 32% of the mass is solid.

Near 1220 °C, the last liquid contains about 24 wt% Ni. When it disappears, the equilibrium solid has reached the overall 35 wt% Ni. All grains are α with uniform composition; the alloy remains single-phase on further cooling.

Why the earlier solid must change

The first α formed at about 46 wt% Ni, yet the final equilibrium α contains 35 wt% Ni. Existing solid must exchange atoms as new solid forms. Enough copper must enter, and nickel must redistribute, for each part of α to match the current solidus composition.

Diffusion in solids is much slower than in liquids. Very slow cooling allows this adjustment. At ordinary casting rates, solid-state diffusion may lag behind the changing equilibrium endpoints.

Coring records the freezing history

When adjustment is incomplete, early solid near a grain's center stays nickel-rich. Later layers formed from a more copper-rich liquid are richer in copper. This composition gradient within a grain is coring.

A cored grain can still be α throughout. Its changing composition does not by itself create a second crystal phase. A microscope or composition scan can reveal a history that the final equilibrium phase label does not show.

Equilibrium coolingCooling with coring
Existing α keeps changing compositionEarlier α retains more of its initial composition
Final α is uniform at the overall compositionNickel-rich centers and copper-rich outer regions remain
Freezing ends at the equilibrium solidusFreezing ends below the equilibrium solidus
Reheating and properties

Copper-rich regions in a cored alloy can begin melting below the equilibrium solidus for the overall composition. Thin liquid regions near boundaries reduce the load-carrying ability of the solid. Homogenization holds the alloy hot while it stays solid, allowing diffusion to smooth out the concentration differences. The temperature must avoid melting the segregated regions.

Mixing copper and nickel also gives solid-solution strengthening. Solute atoms make dislocation motion harder, raising tensile strength and hardness above the pure-metal ends, with a maximum at an intermediate composition. Ductility reaches a minimum at an intermediate composition. A 75 wt% Cu–25 wt% Ni cupronickel alloy is still one α phase: strengthening does not require a second phase to appear.

Key Takeaways

  • The first α in 35 wt% Ni Cu–Ni is nickel-rich, and later solid is richer in copper.
  • Equilibrium cooling needs diffusion through the existing solid.
  • Coring leaves a composition gradient within grains when solid diffusion cannot keep up.
  • Copper-rich regions can melt before the equilibrium solidus is reached on reheating.
  • Homogenization uses solid-state diffusion to reduce coring.
  • Solid-solution strengthening can raise strength while reducing ductility.
3

Interpret eutectic systems and other invariant reactions

Limited solid solubility gives alloys more than one possible solid phase. The lead–tin diagram shows how primary grains and a layered eutectic develop from different cooling paths. Calculations must distinguish whole phases from the microconstituents that contain them. Other diagrams add intermediate compounds and solid-state reactions, which can be identified by tracking the phases on each side of a reaction line.

3.1 Read a binary eutectic diagram

Lead and tin mix fully as a liquid but have limited mutual solubility as solids. Their diagram therefore needs two solid-solution labels, α and β. Its central feature is the temperature at which one liquid becomes both solids.

Find the fields and boundaries

The lead-rich α phase has an FCC structure. The tin-rich β phase has the tetragonal structure of white tin. Both contain some of the other element, so α is not pure lead and β is not pure tin.

The diagram has six fields: L, α, β, α + L, β + L and α + β. Pure lead melts at 327 °C and pure tin at 232 °C. Two liquidus branches descend from those endpoints and meet at 61.9 wt% Sn and 183 °C.

The solid solutions next to the pure-component ends are terminal solid solutions. A solvus bounds each solid's solubility: crossing from α into α + β produces a second solid phase without producing liquid. The solidus instead separates all-solid material from solid plus liquid.

At 183 °C, α holds at most 18.3 wt% Sn. At the other end of the same horizontal line, β contains 97.8 wt% Sn, meaning 2.2 wt% Pb. As temperature falls, the terminal solid solubilities decrease along the solvus lines.

Write the eutectic reaction

The meeting point of the liquidus branches is the eutectic point. On cooling through it,

L(61.9 wt% Sn)→α(18.3 wt% Sn)+β(97.8 wt% Sn).

Heating reverses the reaction. All three phases coexist at 183 °C, so the constant-pressure binary phase rule gives zero degrees of freedom. The horizontal eutectic isotherm extends from 18.3 to 97.8 wt% Sn. It is a reaction line, not an area containing a new phase called “eutectic.”

No liquid is stable below 183 °C in this system. Exactly eutectic liquid freezes at that one temperature. Other compositions generally begin freezing earlier and finish at the eutectic temperature if liquid remains to reach it.

Use three test points

At 200 °C, 10 wt% Sn is all α, while 61.9 wt% Sn is all liquid. At 150 °C, a 40 wt% Sn alloy lies in α + β. The tie-line endpoints are about 11 and 98 wt% Sn, so

Wα=98−4098−11≈0.67,Wβ≈0.33.

The α composition is 11 wt% Sn, not the 67% mass fraction. These numbers answer different questions.

Connect the map to melting behavior

Eutectic compositions are useful when a narrow melting interval is wanted. Traditional solder near 63 wt% Sn and 37 wt% Pb is close to the Pb–Sn eutectic and melts near 183 °C. Lead-free SAC305, Sn–3.0Ag–0.5Cu, is a three-component near-eutectic alloy with a melting range of about 217–220 °C.

Aluminum–silicon provides another binary example: its eutectic is near 12.6 wt% Si and 577 °C. Near-eutectic casting compositions combine relatively low melting temperature with a narrow freezing interval, helping liquid metal fill a mold.

Key Takeaways

  • Pb–Sn contains liquid and two terminal solid solutions, lead-rich α and tin-rich β.
  • A solvus separates one solid phase from two solid phases.
  • The Pb–Sn eutectic is 61.9 wt% Sn at 183 °C.
  • The eutectic reaction converts liquid into two solid phases at a fixed temperature.
  • Phase composition and phase mass fraction are different quantities.

3.2 Predict the microstructures of eutectic-system alloys

Two alloys can contain the same phases but look different under a microscope. In a eutectic system, that difference depends on whether a solid formed before the eutectic reaction, and whether the alloy later crossed a solvus.

Four cooling paths

A very dilute alloy, such as Pb–1 wt% Sn, freezes through α + L into α grains and stays within the room-temperature α solubility limit. Its final structure is single-phase α.

Pb–10 wt% Sn also freezes completely to α. Further cooling crosses the solvus, so β particles form inside α grains and along grain boundaries. This β forms by a solid-state change after freezing; it is not evidence that eutectic liquid was present.

At exactly 61.9 wt% Sn, liquid remains until 183 °C. It then becomes a eutectic structure of alternating α and β layers, or lamellae. Lead and tin redistribute over short distances at the advancing growth front, supplying the neighboring layers. Just below 183 °C,

Wα=97.8−61.997.8−18.3≈0.45,Wβ≈0.55.

For a hypoeutectic alloy between 18.3 and 61.9 wt% Sn, primary α grows before 183 °C. The remaining liquid becomes eutectic. A hypereutectic alloy between 61.9 and 97.8 wt% Sn instead forms primary β, followed by eutectic.

Calculate microconstituents above the reaction

Consider 50 wt% Sn. Just above 183 °C, α contains 18.3 wt% Sn and liquid contains 61.9 wt% Sn. The liquid's mass becomes the eutectic mass, so

We=WL=50−18.361.9−18.3=31.743.6≈0.727.

Primary α makes up the remaining 0.273. The final microconstituents are therefore about 73% eutectic and 27% primary α.

For 80 wt% Sn, use the right-side endpoints: primary β has 97.8 wt% Sn and the remaining liquid has 61.9 wt% Sn. The primary β fraction is (80−61.9)/(97.8−61.9)≈0.50, leaving about 50% eutectic.

Calculate phases below the reaction

For the 50 wt% Sn alloy just below 183 °C, use the full α + β tie line:

Wα=97.8−5097.8−18.3≈0.601,Wβ≈0.399.

Total α includes both the primary grains and the thin α layers inside eutectic. Subtract the primary share to find eutectic α as a fraction of the entire alloy:

0.601−0.273≈0.328.
Requested quantityEndpoints for 50 wt% Sn near 183 °C
Primary α and eutectic18.3 and 61.9 wt% Sn, just above
Total α and total β18.3 and 97.8 wt% Sn, just below

Primary α and eutectic α are the same phase in different microconstituents. Calling all α “primary” misses the α formed during the reaction. Calling all solid “eutectic” misses the grains that formed earlier. On further cooling, phase compositions change along the solvus lines, while the primary-versus-eutectic division remains practically unchanged.

Key Takeaways

  • A dilute alloy can remain one phase or form a second phase after crossing a solvus.
  • Exactly eutectic liquid produces a layered two-phase microconstituent.
  • Hypoeutectic alloys form primary α; hypereutectic alloys form primary β.
  • The liquid fraction just above the eutectic temperature becomes the eutectic fraction.
  • Total α includes primary α and the α inside eutectic.
  • Choose tie-line endpoints according to whether the question asks for phases or microconstituents.

3.3 Recognize intermediate phases and other invariant reactions

A diagram can contain more than terminal solid solutions and a eutectic. To interpret additional fields, identify whether each label names one phase, a compound, or a mixture, then track what changes across each reaction line.

Intermediate phases and compounds

An intermediate solid solution occupies a composition range away from both pure-component ends. It remains one phase. In copper–zinc, α is terminal, while β, γ, δ and ε are intermediate phases. Cartridge brass near 70 wt% Cu–30 wt% Zn is single-phase α; Muntz metal near 60 wt% Cu–40 wt% Zn contains α and β.

An intermetallic compound has a definite chemical formula and a very narrow composition range. Its field can look like a vertical line. Mg₂Si and Fe₃C are examples. Such compounds are often hard and brittle.

A formula counts atoms, so it does not directly give weight percent. For Fe₃C, carbon is one of four atoms, or 25 at%. Its mass percentage is

10012.0113(55.845)+12.011≈6.7 wt% C.

The difference comes from iron atoms being much heavier than carbon atoms. The conventional diagram endpoint is 6.70 wt% C.

Read what reacts on cooling

At a binary invariant line, three phases coexist. Examine the phases consumed and produced as temperature falls:

ReactionCooling formIdentifying change
EutecticL→α+βOne liquid becomes two solids
Eutectoidγ→α+βOne solid becomes two solids
PeritecticL+α→βLiquid and one solid form a different solid
Peritectoidα+β→γTwo solids form a different solid

The product labels depend on the system. In steel, the eutectoid is austenite turning into ferrite and cementite at 727 °C. The iron–carbon peritectic is δ+L→γ at 1493 °C, near 0.17 wt% C. The composition of the new γ lies between those of its reacting liquid and δ.

Reversing the temperature path reverses the reaction. A peritectic product can therefore decompose on heating into a liquid and a different solid. The word “melting” alone does not tell you which solid remains.

Track composition through a transformation

A congruent transformation keeps the compositions of the phases unchanged. Pure copper melting is congruent: both solid and liquid are pure Cu. Pure iron changing from BCC to FCC at 912 °C is also congruent; its structure changes but its composition does not.

An incongruent transformation changes at least one phase composition. Eutectic, eutectoid and peritectic reactions have different parent and product compositions. Most alloys also have different liquid and solid compositions while melting.

A compound that melts congruently can serve as a component for the adjacent portions of its diagram. Each side can then be read as a simpler binary system. A narrow intermediate field is still a phase field; its location between the pure ends does not make it a mixture of those terminal phases.

Key Takeaways

  • An intermediate solid solution is one phase over a range away from pure-component ends.
  • A compound formula fixes atomic proportions; weight percent requires atomic masses.
  • Eutectic and eutectoid reactions differ in whether the starting phase is liquid or solid.
  • A peritectic consumes a liquid and a solid to form a different solid.
  • Congruent transformations preserve phase compositions.
4

Apply the iron–iron carbide diagram to steels and cast irons

Carbon changes the phases and structures that iron develops during cooling. The iron–iron carbide map connects ferrite, austenite and cementite to pearlite in steels and the eutectic in cast irons. Read its key temperatures, then calculate phases and microconstituents with the appropriate tie lines. The same map also shows why carbon content alone is insufficient when alloy additions, graphite formation or rapid cooling change the path.

4.1 Read the iron–iron carbide diagram

Iron changes crystal structure with temperature, and each structure holds a different amount of carbon. The iron–iron carbide diagram combines these changes with carbide formation to explain the phases in steels and cast irons.

Name the phases first

Pure iron is BCC α-ferrite below 912 °C, FCC austenite from 912 to 1394 °C, and BCC δ-ferrite from 1394 °C to melting at 1538 °C. These are allotropic changes: one element changes crystal structure.

Carbon is an interstitial solute in iron. The FCC interstitial sites available in austenite accommodate much more carbon than those in BCC ferrite.

PhaseStructure and carbon contentMechanical or magnetic character
α-ferriteBCC; maximum 0.022 wt% C at 727 °CSoft and ductile; magnetic below about 768 °C
Austenite, γFCC; maximum 2.14 wt% C at 1147 °CNonmagnetic; unstable below 727 °C in plain-carbon steel
Cementite, Fe₃CCarbide at 6.70 wt% CVery hard and brittle

The horizontal axis ends at Fe₃C, not pure carbon. Iron and iron carbide act as the two components. Cementite is chemically distinct from graphite, which is pure carbon.

Recognize the metastable map

Cementite can slowly decompose into iron and graphite. At room temperature it persists for extremely long periods; at about 650–700 °C decomposition can take years. The Fe–Fe₃C map is therefore a metastable diagram, widely useful for steel even though iron plus graphite is the lower-energy alternative.

Following this map means following the carbide-forming path. It does not identify which cast irons instead form graphite.

Locate the reactions and boundaries

Three invariant reactions organize the diagram:

  • At 1493 °C, the peritectic is δ+L→γ.
  • At 1147 °C and 4.30 wt% C, the eutectic is L→γ+Fe3C.
  • At 727 °C and 0.76 wt% C, the eutectoid is γ→α+Fe3C.

A1 is the horizontal eutectoid line. A3 separates γ from α + γ on the low-carbon side; it falls from 912 °C at pure iron to 727 °C at the eutectoid. Acm separates γ from γ + Fe₃C on the higher-carbon side. A hypoeutectoid steel becomes fully austenitic when heated into γ above A3.

Classify and read an alloy

Commercially pure iron contains less than about 0.008 wt% C. Steels span about 0.008–2.14 wt% C, and cast irons occupy the higher-carbon range up to 6.70 wt% C; most cast irons contain 3.0–4.5 wt% C. Within steel, compositions below 0.76 wt% C are hypoeutectoid, exactly 0.76 wt% C is eutectoid, and higher compositions are hypereutectoid.

A 0.20 wt% C steel at 1000 °C is all γ. At 600 °C it contains α and Fe₃C. A 1.20 wt% C steel at 760 °C contains γ and Fe₃C between A1 and Acm. The 2.14 wt% carbon capacity belongs to high-temperature γ, so it cannot be assigned to room-temperature ferrite.

Key Takeaways

  • Ferrite is BCC; austenite is FCC and dissolves much more carbon.
  • The Fe–Fe₃C diagram ends at cementite, 6.70 wt% C.
  • Cementite is metastable and differs from graphite.
  • The eutectoid is 0.76 wt% C at 727 °C; the eutectic is 4.30 wt% C at 1147 °C.
  • A3 and Acm bound the austenite field on opposite sides of the eutectoid.
  • Classify steel relative to 0.76 wt% C before following its cooling path.
  • Carbon solubility values belong to particular phases and temperatures.

4.2 Explain pearlite and hypoeutectoid steels

Pearlite is the layered structure produced when eutectoid austenite transforms. In a lower-carbon steel, some ferrite forms first, so the final steel contains both proeutectoid ferrite and pearlite.

How pearlite grows

A 0.76 wt% C steel cooled slowly through 727 °C changes from austenite into colonies of alternating ferrite and cementite layers. These colonies commonly begin at austenite grain boundaries and grow into the grains.

Growing ferrite can retain only 0.022 wt% C at this temperature. Carbon moves sideways into adjacent cementite, which contains 6.70 wt% C. The short diffusion distances help the two phases grow together as lamellae. Pearlite is a microconstituent, not a third phase.

Within pearlite, the α + Fe₃C tie line gives

Wα=6.70−0.766.70−0.022≈0.89,WFe3C≈0.11.

Ferrite and cementite densities are close, about 7.87 and 7.69 g/cm³, so ferrite layers are roughly eight times as thick as cementite layers. Pearlite is stronger and harder than ferrite, with less ductility.

Follow a hypoeutectoid steel

A 0.40 wt% C steel at 900 °C is all γ. Below A3, proeutectoid ferrite forms, often along γ grain boundaries. Since ferrite holds little carbon, the remaining γ becomes richer in carbon as cooling continues. Just above 727 °C, α contains 0.022 wt% C and γ contains 0.76 wt% C. All remaining γ then becomes pearlite.

To find microconstituents, use this tie line just above A1:

Wp=C0−0.0220.76−0.022,Wα′=0.76−C00.76−0.022.

For 0.40 wt% C, Wp=0.378/0.738≈0.512 and Wα′≈0.488. A 1 kg sample therefore contains about 512 g pearlite and 488 g proeutectoid ferrite.

This pearlite formula applies between 0.022 and 0.76 wt% C. At or below 0.022 wt% C, no eutectoid pearlite forms during equilibrium cooling; ferrite can accommodate the carbon at A1.

Count all ferrite when asked for phases

Just below 727 °C, the phase endpoints are 0.022 and 6.70 wt% C:

Wα=6.70−0.406.70−0.022≈0.943,WFe3C≈0.057.

The 94.3% total ferrite includes the 48.8% proeutectoid ferrite and about 45.5% ferrite inside pearlite. Adding pearlite to total ferrite would count that ferrite twice. The 0.76 endpoint belongs to the parent γ used for microconstituents; the 6.70 endpoint belongs to the cementite phase used for total phases.

Infer composition from a micrograph

The relationship can run backward. If about 60% of a slowly cooled hypoeutectoid steel is pearlite, estimate

C0=0.022+0.60(0.76−0.022)≈0.46 wt% C.

A representative section's area fractions estimate volume fractions. Their use as mass fractions here is close because ferrite and pearlite have nearly equal densities. Within this slow-cooled low-carbon range, increasing carbon increases pearlite, strength and hardness, while lowering ductility.

Key Takeaways

  • Pearlite contains ferrite and cementite in alternating layers.
  • Proeutectoid ferrite forms before the eutectoid reaction in hypoeutectoid steel.
  • Remaining austenite becomes pearlite at 727 °C.
  • Use 0.022 and 0.76 wt% C for hypoeutectoid microconstituent fractions.
  • Use 0.022 and 6.70 wt% C for total phase fractions just below 727 °C.
  • Total ferrite includes ferrite inside pearlite.
  • A pearlite fraction can estimate carbon content in a slowly cooled hypoeutectoid steel.

4.3 Analyze hypereutectoid steels, cast irons and the diagram's limits

Above the eutectoid composition, cementite forms before pearlite. Cast irons add an earlier eutectic reaction during freezing. In both cases, follow the cooling sequence before choosing which fractions to calculate.

Hypereutectoid steel: cementite first

A 1.20 wt% C steel is all γ at about 950 °C. Below Acm, proeutectoid cementite forms, often at γ grain boundaries. As this carbon-rich phase grows, the remaining γ loses carbon until it reaches 0.76 wt% C at 727 °C. That γ becomes pearlite, leaving pearlite colonies bordered by cementite.

Just above A1, use the γ–Fe₃C endpoints:

WFe3C′=C0−0.766.70−0.76,Wp=6.70−C06.70−0.76.

For 1.20 wt% C, proeutectoid cementite is 0.44/5.94≈0.074 and pearlite is about 0.926. Below A1, total cementite uses a different tie line:

WFe3C=1.20−0.0226.70−0.022≈0.176.

About 0.176−0.074=0.102 of the entire steel is cementite inside pearlite. A continuous boundary network of brittle cementite reduces toughness, which motivates heat treatments that change its form.

At 2.14 wt% C, the upper steel boundary, proeutectoid cementite reaches only (2.14−0.76)/5.94≈0.23. A slowly cooled steel showing 40% proeutectoid material cannot have that share as cementite; it points to proeutectoid ferrite on the lower-carbon side.

Cast iron: start at the eutectic

On the Fe–Fe₃C path, liquid at 4.30 wt% C transforms at 1147 °C into γ of 2.14 wt% C and cementite of 6.70 wt% C. This eutectic microconstituent is ledeburite.

A 3.0 wt% C iron forms primary γ before reaching 1147 °C. Just above the reaction,

Wγ′=4.30−3.04.30−2.14≈0.60,We≈0.40.

The remaining 40% liquid becomes ledeburite. As cooling continues, γ rejects carbon and additional cementite forms. At 727 °C, the remaining γ becomes pearlite. Thus ledeburite begins as γ + Fe₃C, but its γ does not survive to room temperature on this slow-cooled path.

Silicon and slow cooling favor graphite formation in cast irons. When graphite forms, the iron–graphite diagram describes that path; a carbide-only calculation cannot assign the graphite amount.

Know when the numbers change

Alloying shifts the eutectoid point. Nickel and manganese lower its temperature; molybdenum, silicon, tungsten and titanium raise it. Most common alloying additions lower its carbon composition. A plain-carbon value such as 0.76 wt% C cannot simply be carried into every alloy steel.

Cooling rate matters too. Less diffusion time gives finer pearlite, and rapid quenching can produce martensite, which the equilibrium map does not show. The lever rule's equilibrium fractions do not describe a quenched steel. A useful analysis therefore names the alloy system and cooling path, identifies each reaction, and keeps microconstituent fractions separate from total phase fractions.

Key Takeaways

  • Hypereutectoid steel forms proeutectoid cementite and then pearlite.
  • Use 0.76 and 6.70 wt% C for its microconstituent fractions near A1.
  • Total cementite also counts cementite within pearlite.
  • Ledeburite forms from eutectic liquid at 1147 °C on the Fe–Fe₃C path.
  • Cast-iron analysis begins with the primary/eutectic division, then follows solid-state changes.
  • Graphite formation, alloy additions and fast cooling change which diagram or method applies.
  • Equilibrium fractions cannot predict quenched microstructures.

Phase Diagrams examples

4 Walkthroughs

1

Read what a phase diagram tells you

11 steps
Build a precise description of a material, then connect the axes and phase rule to equilibrium fields.
  1. 1
    IntroductionFrom an alloy sample to an equilibrium map

    A metal sample has a chemical recipe, a set of phases and a microstructure. Each describes a different aspect of the same material.

    Start by deciding what counts as a phase. Then read how temperature, pressure and composition place a sample on a diagram. These choices determine whether the next question needs one composition or separate compositions for coexisting phases.

  2. 2
    ExampleOne ingredient can make two phases

    A container holds ice and liquid water. Its only chemical component is water, but the solid and liquid have different physical structures, so they are two phases.

    Now consider a uniform solid Cu–Ni solution. It has two components, copper and nickel, in one crystalline phase. Counting ingredients cannot replace identifying the uniform physical and chemical regions.

  3. 3
    ExplanationGrains and phases answer different questions

    A grain is one crystal orientation within a solid. Many differently oriented grains can share the same composition and crystal structure, so they belong to the same phase.

    A microconstituent is a recognizable structural region. Pearlite is one such region containing two phases in layers. A micrograph therefore needs more than a count: identify the phases and describe how they are arranged.

  4. 4
    ExampleUse the total solution mass

    At 20 °C, 204 g sugar dissolves in 100 g water. The solution's total mass is 304 g, so its sugar content is

    100(204/304)≈67 wt%.

    The solubility limit belongs to that temperature. A 75 wt% mixture cannot keep all its sugar dissolved there: saturated syrup coexists with solid sugar. The 204 g per 100 g water ratio uses a different denominator from weight percent.

  5. 5
    ChallengeSeparate atoms from mass

    A solid compound is Fe₃C. Without using atomic masses, what carbon percentage can you find, and why can you not call it a weight percentage?

    ---reveal---

    Carbon is one of four atoms, so the composition is 25 at% C. Weight percent requires the mass contribution of each kind of atom. Iron and carbon have different atomic masses, so their atom shares and mass shares differ.

  6. 6
    ExplanationChoose the right pair of axes

    A unary water diagram varies temperature and pressure. At 1 atm, heating takes ice through melting at 0 °C and water through boiling at 100 °C.

    A binary alloy diagram usually fixes pressure and varies temperature vertically and composition horizontally. Read whether that composition axis uses wt% or at% before locating the sample; the same numerical value on those scales usually means a different alloy.

  7. 7
    Key InsightThe map has no clock

    At equilibrium, phases and their compositions and amounts remain constant at the given conditions. A metastable state can persist because the route to a lower-energy state is very slow.

    A diagram maps equilibrium states, not the time needed to reach them. A rapidly cooled alloy may retain a different structure because atoms have too little time to move. Temperature and composition alone do not specify that cooling history.

  8. 8
    ExampleRead the phase rule inside a field

    For a binary system at fixed pressure,

    F=3−P.

    Inside a two-phase field, P=2, so one intensive variable remains independent. Choose the temperature and the diagram fixes both phase compositions at the horizontal tie-line endpoints.

    You can still vary overall composition along that tie line by changing phase amounts. Amounts are not additional degrees of freedom in this rule.

  9. 9
    ChallengeRecognize the invariant condition

    Liquid and two solids coexist in a binary alloy at fixed pressure. Can temperature change freely while all three remain in equilibrium?

    ---reveal---

    No. Three phases give F=3−3=0. The temperature and phase compositions are fixed at that invariant reaction. Its horizontal line represents a fixed-temperature equilibrium, even though the reacting phase amounts can change.

  10. 10
    ChallengeExplain two samples on one tie line

    Two samples lie at the same temperature inside the same α + β field, but have different overall compositions. Must they have different phases or different phase compositions?

    ---reveal---

    Neither is required. Both contain α and β at the same endpoint compositions. Different amounts of α and β account for the different overall compositions. This uses both the meaning of a phase and the one-degree-of-freedom rule for two-phase equilibrium.

  11. 11
    RecapDecide what information you need next

    Read the axes and locate the sample before calculating. In one phase, its composition equals the overall composition and its fraction is 1.

    In two phases, the overall value is an average: obtain each phase composition from the endpoints and then find their amounts. Describe grains and microconstituents separately when the question concerns the structure visible under a microscope.

2

Calculate an alloy’s phases during freezing

14 steps
Work through a Cu–Ni tie line, check mass balance, and explain the diffusion needed to follow equilibrium cooling.

Save this lesson to follow every Walkthrough step by step.

  1. 1
    IntroductionFollow one casting through freezing
  2. 2
    ExplanationUse the isomorphous lens
  3. 3
    ExampleKeep overall composition fixed
  4. 4
    ChallengeInterpret a single-phase reading
  5. 5
    ExampleRead the endpoints before the arms
  6. 6
    ExampleCalculate the solid share
  7. 7
    ExampleConvert fractions into kilograms
  8. 8
    ChallengeDistinguish mass from volume
  9. 9
    ExplanationMake the early solid adjust
  10. 10
    ConnectionRead the record inside a cored grain
  11. 11
    ChallengeChoose a reason for homogenization
  12. 12
    Key InsightStrength can rise within one phase
  13. 13
    ChallengeCheck a claim against composition and history
  14. 14
    RecapA reading, a balance and a cooling history
3

Track primary grains and eutectic layers

15 steps
Follow Pb–Sn cooling, calculate phases and microconstituents separately, and recognize other invariant reaction types.

Save this lesson to follow every Walkthrough step by step.

  1. 1
    IntroductionThe same phases can form different structures
  2. 2
    ExplanationPlace the eutectic and solid endpoints
  3. 3
    ExampleWrite the reaction with phase identities
  4. 4
    ChallengeIdentify a solid-state boundary
  5. 5
    ExplanationCompare the dilute and eutectic paths
  6. 6
    ExampleLet primary α form first
  7. 7
    ExampleTurn the remaining liquid into a eutectic amount
  8. 8
    ExampleCount α everywhere it occurs
  9. 9
    ChallengeRead the tin-rich side
  10. 10
    ExplanationRecognize an interior phase field
  11. 11
    ConnectionChange the parent phase to get a eutectoid
  12. 12
    ExplanationRead a peritectic from its reactants
  13. 13
    ChallengeSeparate structure change from composition change
  14. 14
    ChallengeAudit a two-number description
  15. 15
    RecapMatch the tie line to the question
4

Calculate pearlite, carbide and cast-iron constituents

19 steps
Read the Fe–Fe₃C map and work from a cooling path to separate microconstituent fractions from total phases.

Save this lesson to follow every Walkthrough step by step.

  1. 1
    IntroductionCarbon controls which constituent appears first
  2. 2
    ExplanationMatch structure to carbon capacity
  3. 3
    ExampleLocate three reactions and three boundary names
  4. 4
    ChallengeChoose the correct pure-iron structure
  5. 5
    ExplanationLet neighboring layers share carbon
  6. 6
    ExampleCalculate the phases within pearlite
  7. 7
    ExampleFollow a 0.40 wt% C steel below A3
  8. 8
    ExampleUse the parent austenite endpoint
  9. 9
    ChallengeCount ferrite within the pearlite too
  10. 10
    ConnectionRead composition backward from pearlite
  11. 11
    ExplanationCross Acm on the high-carbon side
  12. 12
    ExampleSeparate early carbide from all carbide
  13. 13
    ChallengeCheck a large proeutectoid share
  14. 14
    ExampleBegin cast iron at 1147 °C
  15. 15
    ConnectionFollow the austenite after freezing
  16. 16
    Key InsightKeep the system and cooling path attached
  17. 17
    ChallengeCheck the low-carbon limit before using the formula
  18. 18
    ChallengeChoose two balances for one high-carbon steel
  19. 19
    RecapChoose the structure before the fraction

Phase Diagrams practice questions

40 Practice Questions in 4 sets

Set 1: Follow cooling and separate constituents10 Practice Questions

Question 1 of 10

A 100 g Cu–Ni sample contains 20 g Ni and 80 g Cu. Atomic masses are 58.69 g/mol Ni and 63.55 g/mol Cu. About what atom percent is nickel?
  1. 20.0 at%
  2. 18.8 at%
  3. 21.3 at%
  4. 25.0 at%
Show answerHide answer
Answer: C
Convert the masses to moles: nickel contributes about 0.341 mol and copper about 1.259 mol. Nickel is 0.3410.341+1.259, or about 21.3 at%. The 20.0% value is the weight percent; the lighter nickel atoms give a slightly larger atom share than mass share.

Question 2 of 10

Ice is heated at a constant pressure below water’s triple-point pressure. What stable phase follows the ice?
  1. Water vapor
  2. Liquid water
  3. Ice and liquid water
  4. Liquid water and vapor
Show answerHide answer
Answer: A
Below the triple-point pressure, heating crosses from the ice region into the vapor region, so the change is sublimation. A stable liquid-water field is unavailable at that pressure. Applying the familiar 1 atm melting sequence would use the wrong pressure path through the water diagram.

Question 3 of 10

A Cu–Ni alloy starts melting at 1210 °C and becomes completely liquid at 1245 °C. What do those temperatures identify?
  1. 1210 °C liquidus; 1245 °C solidus
  2. 1210 °C solvus; 1245 °C solidus
  3. 1210 °C solidus; 1245 °C solvus
  4. 1210 °C solidus; 1245 °C liquidus
Show answerHide answer
Answer: D
On heating, the solidus marks the first liquid and the liquidus marks the disappearance of the last solid. The interval between them contains solid and liquid together. Swapping the two names confuses heating order with the fact that the liquidus is the upper boundary of the two-phase field.

Question 4 of 10

A Cu–Ni grain has a nickel-rich center and copper-rich outer layers after casting. What explains this pattern?
  1. Early solid reached the final alloy composition.
  2. Early solid retained its nickel enrichment.
  3. Late solid formed from nickel-rich pure liquid.
  4. Late solid converted into a second crystal phase.
Show answerHide answer
Answer: B
The first solid is richer in nickel, and later solid grows from liquid that becomes richer in copper. If solid-state diffusion cannot keep up, the center retains more of its early composition and coring remains. A new crystal phase is unnecessary; a single α grain can contain this composition gradient.

Question 5 of 10

What phases form when eutectic Pb–Sn liquid freezes at 183 °C?
  1. Lead-rich α and tin-rich β
  2. Pure lead and pure tin
  3. Lead-rich α and remaining liquid
  4. Tin-rich β and remaining liquid
Show answerHide answer
Answer: A
The eutectic liquid transforms into the two solid solutions α and β. Their compositions at the reaction are 18.3 and 97.8 wt% Sn, so neither is a pure element. Remaining liquid belongs to the partly completed reaction, not the fully frozen eutectic product requested here.

Question 6 of 10

A 45 wt% Sn alloy cools slowly through 183 °C. What is its approximate eutectic mass fraction? Use 18.3, 61.9 and 97.8 wt% Sn.
  1. 0.388
  2. 0.612
  3. 0.664
  4. 0.336
Show answerHide answer
Answer: B
The liquid remaining just above 183 °C becomes eutectic, giving 45−18.361.9−18.3≈0.612. The complementary 0.388 is primary α. Using the endpoint 97.8 instead would calculate a total solid-phase fraction, mixing up phases with microconstituents.

Question 7 of 10

A 75 wt% Sn alloy cools slowly to just below 183 °C. About what mass fraction of the whole alloy is β inside the eutectic? Use 18.3, 61.9 and 97.8 wt% Sn.
  1. 0.365
  2. 0.635
  3. 0.713
  4. 0.348
Show answerHide answer
Answer: D
Primary β is 75−61.997.8−61.9≈0.365. Total β below the reaction is 75−18.397.8−18.3≈0.713, so β within eutectic is about 0.348, or 0.35. The 0.635 fraction is the whole eutectic and includes its α as well as its β.

Question 8 of 10

What is the crystal structure of pure iron at 1200 °C?
  1. BCC α-ferrite
  2. BCC δ-ferrite
  3. FCC austenite
  4. Orthorhombic cementite
Show answerHide answer
Answer: C
At 1200 °C, pure iron lies between its 912 °C and 1394 °C structural changes, so it is FCC austenite. Both ferrite forms are BCC but occupy different temperature ranges. Choosing δ-ferrite places the alloy in the higher-temperature region above 1394 °C too early.

Question 9 of 10

A representative micrograph of slowly cooled hypoeutectoid steel shows 35% pearlite by area. Treat the area fraction as a mass-fraction estimate. What carbon content and total cementite fraction just below 727 °C follow?
  1. 0.280 wt% C; 0.039 cementite
  2. 0.266 wt% C; 0.035 cementite
  3. 0.280 wt% C; 0.350 cementite
  4. 0.502 wt% C; 0.072 cementite
Show answerHide answer
Answer: A
The inferred composition is 0.022+0.35(0.76−0.022)≈0.280 wt% C. Total cementite is then 0.280−0.0226.70−0.022≈0.039. Multiplying 0.35 by 0.76 alone omits the carbon retained by the proeutectoid ferrite.

Question 10 of 10

A 3.40 wt% C iron follows the Fe–Fe₃C path through 1147 °C. What is the approximate ratio of primary austenite mass to ledeburite mass immediately below the reaction? Use 2.14, 4.30 and 6.70 wt% C.
  1. 1.40 : 1
  2. 1.54 : 1
  3. 0.71 : 1
  4. 0.46 : 1
Show answerHide answer
Answer: C
Primary austenite is 4.30−3.404.30−2.14≈0.417, leaving 0.583 liquid to become ledeburite. Their mass ratio is therefore 0.417/0.583≈0.71. Using 6.70 as the second endpoint would count total austenite after the eutectic, including austenite within ledeburite.
Set 2: Read phases and calculate first fractions10 Practice Questions

Save this lesson to see every answer and practice every set.

Question 1 of 10

A two-phase solid contains 0.60 mass fraction α and 0.40 mass fraction β. Their densities are 9.0 and 6.0 g/cm³. What is the volume fraction of α?
  1. 0.60
  2. 0.50
  3. 0.69
  4. 0.40
Show answerHide answer

Save this lesson to see this answer.

Question 2 of 10

A Pb–Sn alloy crosses from α into α + β during cooling, with no liquid present. What boundary has it crossed?
  1. A liquidus
  2. A solidus
  3. A eutectic isotherm
  4. A solvus
Show answerHide answer

Save this lesson to see this answer.

Question 3 of 10

An invariant reaction consumes one solid and produces two different solids during cooling. What kind of reaction is it?
  1. Eutectoid
  2. Eutectic
  3. Peritectic
  4. Peritectoid
Show answerHide answer

Save this lesson to see this answer.

Question 4 of 10

Why does austenite dissolve much more carbon than ferrite?
  1. Its iron atoms have a much larger atomic mass.
  2. It places carbon on regular iron lattice sites.
  3. Its interstitial sites accommodate carbon better.
  4. Its carbon atoms have a smaller atomic radius.
Show answerHide answer

Save this lesson to see this answer.

Question 5 of 10

A slowly cooled 0.30 wt% C steel is examined just below 727 °C. Approximately what fraction of the entire steel is ferrite inside pearlite? Use 0.022, 0.76 and 6.70 wt% C.
  1. 0.38
  2. 0.62
  3. 0.96
  4. 0.34
Show answerHide answer

Save this lesson to see this answer.

Question 6 of 10

A chemically uniform copper–nickel solid has 200 grains, all FCC with the same composition. How many phases are present?
  1. Two phases
  2. One phase
  3. One phase per grain
  4. One phase per element
Show answerHide answer

Save this lesson to see this answer.

Question 7 of 10

How many degrees of freedom does a binary two-phase equilibrium have at constant pressure?
  1. One
  2. Zero
  3. Two
  4. Three
Show answerHide answer

Save this lesson to see this answer.

Question 8 of 10

What phases occupy the region between the Cu–Ni liquidus and solidus?
  1. Liquid and pure nickel
  2. Two different α solid solutions
  3. α solid solution and pure copper
  4. Liquid and α solid solution
Show answerHide answer

Save this lesson to see this answer.

Question 9 of 10

A 37.0 wt% Ni alloy at 1250 °C has liquid at 31.5 wt% Ni and α at 42.5 wt% Ni. What fraction of its mass is α?
  1. 0.13
  2. 0.87
  3. 0.50
  4. 0.37
Show answerHide answer

Save this lesson to see this answer.

Question 10 of 10

A 1.50 wt% C plain-carbon steel cools slowly from austenite to just below 727 °C. What are its approximate proeutectoid and total cementite mass fractions?
  1. 0.221 proeutectoid; 0.125 total
  2. 0.125 proeutectoid; 0.221 total
  3. 0.125 proeutectoid; 0.096 total
  4. 0.875 proeutectoid; 0.221 total
Show answerHide answer

Save this lesson to see this answer.

Set 3: Use balances and interpret reaction paths10 Practice Questions

Save this lesson to see every answer and practice every set.

Question 1 of 10

At a fixed temperature, a solute has a solubility of 150 g per 100 g solvent. What is its weight percentage in the saturated solution?
  1. 150 wt%
  2. 40 wt%
  3. 67 wt%
  4. 60 wt%
Show answerHide answer

Save this lesson to see this answer.

Question 2 of 10

In a fully solid isomorphous alloy, what changes as overall composition varies across the diagram?
  1. The number of solid phases at every point
  2. The solid phase into alternating pure elements
  3. The composition of the same solid phase
  4. The solid composition while remaining pure
Show answerHide answer

Save this lesson to see this answer.

Question 3 of 10

A 1.8 kg Cu–Ni alloy at 1250 °C contains 0.9 kg solid α. The tie-line endpoints are 31.5 and 42.5 wt% Ni. A new 2.0 kg charge will have the same overall composition. How much more nickel must the new charge contain?
  1. 0.074 kg Ni
  2. 0.063 kg Ni
  3. 0.085 kg Ni
  4. 0.100 kg Ni
Show answerHide answer

Save this lesson to see this answer.

Question 4 of 10

Two castings have the same overall Cu–Ni composition. One has uniform grains; the other has coring. Why can their reheating behavior differ?
  1. The cored casting contains more nickel overall.
  2. The cored casting has lower-melting local regions.
  3. The uniform casting retains more liquid at room temperature.
  4. The uniform casting lacks a solid-solution phase.
Show answerHide answer

Save this lesson to see this answer.

Question 5 of 10

At 150 °C, α contains 11 wt% Sn and β contains 98 wt% Sn. Two alloys contain 25 and 55 wt% Sn. How do their equilibrium phases compare?
  1. Same phase compositions; more β in 55 wt% Sn.
  2. Same phase compositions; more α in 55 wt% Sn.
  3. Same phase fractions; richer β in 55 wt% Sn.
  4. Same phase fractions; richer α in 55 wt% Sn.
Show answerHide answer

Save this lesson to see this answer.

Question 6 of 10

A slowly cooled hypoeutectic Pb–Sn specimen is 40% primary α by mass just below 183 °C. What overall Sn content and total α fraction follow? Use 18.3, 61.9 and 97.8 wt% Sn.
  1. 44.46 wt% Sn; 0.400 total α
  2. 50.24 wt% Sn; 0.598 total α
  3. 44.46 wt% Sn; 0.671 total α
  4. 34.26 wt% Sn; 0.799 total α
Show answerHide answer

Save this lesson to see this answer.

Question 7 of 10

A compound X has 40 wt% B. On heating at an invariant temperature, it produces liquid at 25 wt% B and solid Y at 60 wt% B. What kind of melting occurs, and approximately what fraction becomes liquid?
  1. Congruent; 0.571 liquid
  2. Incongruent; 0.571 liquid
  3. Incongruent; 0.429 liquid
  4. Congruent; 0.429 liquid
Show answerHide answer

Save this lesson to see this answer.

Question 8 of 10

A plain-carbon steel is entirely austenite at high temperature. During slow cooling, ferrite appears before 727 °C. Through what boundary did it leave the austenite field?
  1. A1
  2. Acm
  3. The eutectic isotherm
  4. A3
Show answerHide answer

Save this lesson to see this answer.

Question 9 of 10

Two slowly cooled hypoeutectoid steels contain 0.25 and 0.55 wt% C. How much greater is the pearlite mass fraction of the second steel, and what mechanical trend follows?
  1. About 0.30 greater; generally less ductile.
  2. About 0.41 greater; generally more ductile.
  3. About 0.41 greater; generally less ductile.
  4. About 0.08 greater; generally less ductile.
Show answerHide answer

Save this lesson to see this answer.

Question 10 of 10

An equilibrium-cooled plain-carbon steel is reported to contain 40% proeutectoid constituent by mass. What identity and approximate overall carbon content fit the report?
  1. Ferrite; 0.465 wt% C
  2. Cementite; 3.136 wt% C
  3. Ferrite; 0.317 wt% C
  4. Cementite; 0.465 wt% C
Show answerHide answer

Save this lesson to see this answer.

Set 4: Combine microstructure evidence and calculations10 Practice Questions

Save this lesson to see every answer and practice every set.

Question 1 of 10

At a binary eutectic temperature, α, β and liquid coexist at constant pressure. Different specimens can contain different overall compositions. How is that compatible with zero degrees of freedom?
  1. Phase amounts vary while phase compositions stay fixed.
  2. Phase compositions vary while temperature stays fixed.
  3. Pressure varies while phase compositions stay fixed.
  4. Component count varies while temperature stays fixed.
Show answerHide answer

Save this lesson to see this answer.

Question 2 of 10

At one temperature, a binary α + β alloy has Cα = 20 wt% B and Cβ = 80 wt% B. The phase densities are 8 and 4 g/cm³. What overall composition gives equal phase volumes?
  1. 50 wt% B
  2. 60 wt% B
  3. 40 wt% B
  4. 30 wt% B
Show answerHide answer

Save this lesson to see this answer.

Question 3 of 10

A 3 kg alloy at 1250 °C contains 0.40 mass fraction α, with Cu–Ni endpoints 31.5 and 42.5 wt% Ni. It is mixed with pure copper and re-equilibrated at the same temperature until α is 0.20 of the mass. About how much copper was added?
  1. 0.600 kg
  2. 0.092 kg
  3. 0.394 kg
  4. 0.196 kg
Show answerHide answer

Save this lesson to see this answer.

Question 4 of 10

A Cu–Ni casting is held hot without any local melting until its grain-center and grain-edge compositions become alike. What mechanism removes the coring?
  1. Grain boundaries sweep the solid.
  2. Atoms diffuse through the solid.
  3. Solute forms a second solid phase.
  4. New grains form by recrystallizing.
Show answerHide answer

Save this lesson to see this answer.

Question 5 of 10

A 68 wt% Sn alloy cools slowly through 183 °C. What fraction of its total β belongs to primary β immediately below the reaction? Use 18.3, 61.9 and 97.8 wt% Sn.
  1. About 0.170
  2. About 0.625
  3. About 0.272
  4. About 0.830
Show answerHide answer

Save this lesson to see this answer.

Question 6 of 10

What reaction occurs when liquid and δ-ferrite combine to form austenite on cooling?
  1. Eutectic
  2. Peritectic
  3. Eutectoid
  4. Peritectoid
Show answerHide answer

Save this lesson to see this answer.

Question 7 of 10

A slowly cooled 0.65 wt% C steel has a mass of 5.0 kg. Approximately how much ferrite lies inside pearlite just below 727 °C? Use 0.022, 0.76 and 6.70 wt% C.
  1. 3.78 kg
  2. 4.25 kg
  3. 4.53 kg
  4. 0.47 kg
Show answerHide answer

Save this lesson to see this answer.

Question 8 of 10

A 0.015 wt% C alloy cools in equilibrium through 727 °C. What eutectoid pearlite fraction forms?
  1. About 0.020
  2. About 0.010
  3. About 0.980
  4. Zero
Show answerHide answer

Save this lesson to see this answer.

Question 9 of 10

A 3.60 wt% C iron follows the Fe–Fe₃C path to just below 1147 °C. What is the approximate ratio of total austenite mass to primary austenite mass? Use 2.14, 4.30 and 6.70 wt% C.
  1. 1.00 : 1
  2. 2.10 : 1
  3. 0.68 : 1
  4. 3.09 : 1
Show answerHide answer

Save this lesson to see this answer.

Question 10 of 10

A 3.80 wt% C cast iron follows iron–graphite equilibrium at a temperature where its iron-rich phase contains 0.020 wt% C. The iron-rich phase and graphite have densities of 7.8 and 2.2 g/cm³. What is the approximate graphite volume fraction?
  1. 0.122
  2. 0.038
  3. 0.010
  4. 0.878
Show answerHide answer

Save this lesson to see this answer.

Stuck on your own question? Homework Help

Key Terms

64 Key Terms, each with its definition

A

A1 line
The A1 line is the horizontal eutectoid equilibrium line at 727 °C in the plain-carbon iron–iron carbide phase diagram.
“Remaining austenite becomes pearlite when a slowly cooled steel passes through the A1 line.”
A3 line
The A3 line separates single-phase austenite from ferrite plus austenite on the hypoeutectoid side of the Fe–Fe₃C diagram.
“Proeutectoid ferrite first appears when a cooling hypoeutectoid steel crosses the A3 line.”
Acm line
The Acm line separates single-phase austenite from austenite plus cementite on the hypereutectoid side of the Fe–Fe₃C diagram.
“A hypereutectoid steel begins forming proeutectoid cementite when its cooling path crosses the Acm line.”
Allotropy
Allotropy is the ability of an element to exist in different crystal structures, with temperature determining which structure is stable.
“Iron’s allotropy changes its structure from BCC to FCC at 912 °C and back to BCC at 1394 °C.”
Area fraction
An area fraction is the fraction of a representative section occupied by a phase or constituent, used to estimate its volume fraction.
“A measured pearlite area fraction can estimate carbon content when a slow-cooled steel’s density differences are small.”
Atom percent
Atom percent expresses the number of atoms of one element as a percentage of the total number of atoms in a mixture.
“Carbon accounts for 25 atom percent in Fe₃C because one of every four atoms in the formula is carbon.”
Austenite
Austenite is the FCC solid solution of carbon in iron, called γ, which can dissolve up to 2.14 wt% C at 1147 °C.
“Austenite in a plain-carbon steel transforms as the temperature falls through the eutectoid reaction.”

C

Cast iron
A cast iron is a high-carbon iron alloy above the steel range; the Fe–Fe₃C diagram places that range above about 2.14 wt% C.
“A cast iron at 3.4 wt% C can be followed through the eutectic if it takes the carbide-forming path.”
Cementite
Cementite is iron carbide, Fe₃C, a very hard, brittle, metastable compound represented at 6.70 wt% C on the phase diagram.
“Cementite forms the thin hard layers that alternate with ferrite inside a pearlite colony.”
Component
A component is a chemically distinct ingredient, such as an element or compound, used to specify a material system.
“Copper is one component of a copper–nickel alloy, even when both elements share one solid phase.”
Congruent transformation
A congruent transformation changes physical state or crystal structure without changing the compositions of the participating phases.
“Pure iron’s change from BCC ferrite to FCC austenite is a congruent transformation because it remains pure iron.”
Coring
Coring is a composition gradient within a solidified grain caused by incomplete diffusion as successive layers form from changing liquid.
“Coring in a Cu–Ni casting leaves nickel-rich grain centers and more copper-rich outer regions.”

D

Degrees of freedom
The degrees of freedom count intensive variables that can change independently while the specified equilibrium phases remain present.
“A binary two-phase field at fixed pressure has one degree of freedom, so temperature fixes the phase compositions.”

E

Equilibrium
Equilibrium is the lowest-free-energy state available at fixed temperature, pressure and composition, with phase amounts and compositions constant.
“A slowly cooled alloy approaches equilibrium as diffusion gives its atoms time to redistribute.”
Equilibrium cooling
Equilibrium cooling is cooling slow enough for phase compositions and amounts to keep adjusting to their equilibrium values through diffusion.
“Equilibrium cooling leaves a fully solid Cu–Ni alloy with uniform composition throughout its α grains.”
Eutectic isotherm
A eutectic isotherm is the horizontal reaction line at the temperature where liquid and two solid phases can coexist in a binary system.
“The Pb–Sn eutectic isotherm connects the α and β endpoints at 18.3 and 97.8 wt% Sn at 183 °C.”
Eutectic point
A eutectic point identifies the liquid composition and temperature at which that liquid transforms into two solid phases on cooling.
“The eutectic point in Pb–Sn is located at 61.9 wt% Sn and 183 °C, where the liquidus branches meet.”
Eutectic reaction
A eutectic reaction is an invariant change in which one liquid forms two solid phases on cooling, with the reverse change on heating.
“The Pb–Sn eutectic reaction produces lead-rich α and tin-rich β from liquid at the eutectic composition.”
Eutectic structure
A eutectic structure is the two-solid microconstituent formed during a eutectic reaction, often arranged as alternating layers.
“The eutectic structure surrounding primary α grains contains both thin α layers and thin β layers.”
Eutectoid reaction
A eutectoid reaction is an invariant transformation in which one solid becomes two different solid phases during cooling.
“Steel’s eutectoid reaction changes austenite into ferrite and cementite at 727 °C on the plain-carbon diagram.”
Eutectoid steel
A eutectoid steel has the eutectoid carbon composition, 0.76 wt% C on this diagram, and becomes pearlite during slow cooling through A1.
“A eutectoid steel needs no separate proeutectoid phase before its austenite transforms into pearlite.”

F

Ferrite
Ferrite is the BCC solid solution of carbon in iron; its low-temperature α form dissolves at most 0.022 wt% C at 727 °C.
“Ferrite gives a slowly cooled low-carbon steel a relatively soft, ductile phase surrounding pearlite.”

G

Gibbs phase rule
The Gibbs phase rule relates phase count to independent intensive variables; for a binary system at fixed pressure, it gives F=3−P.
“The Gibbs phase rule gives zero freedom when liquid and two solids coexist at a binary eutectic.”
Graphite
Graphite is a crystalline form of pure carbon that can form in cast irons, providing an alternative to carbon bound in cementite.
“Silicon and slow cooling favor graphite in cast iron, changing which carbon phase must be counted.”

H

Homogenization
Homogenization is a hot solid-state treatment that allows diffusion to reduce composition differences left by solidification.
“Homogenization smooths a cored grain’s composition while the alloy is held below local melting temperatures.”
Hume–Rothery rules
The Hume–Rothery rules are empirical guidelines linking substitutional solubility to atomic size, crystal structure, electronegativity and valence.
“Copper and nickel satisfy the size and structure features emphasized by the Hume–Rothery rules.”
Hypereutectic alloy
A hypereutectic alloy has an overall composition above the eutectic composition on the stated solute scale, on the right side of that point.
“A Pb–Sn alloy at 80 wt% Sn is hypereutectic and develops primary β followed by a eutectic structure.”
Hypereutectoid steel
A hypereutectoid steel has more than the eutectoid carbon content and forms proeutectoid cementite before the remaining austenite transforms.
“A 1.20 wt% C hypereutectoid steel develops cementite at grain boundaries before pearlite forms.”
Hypoeutectic alloy
A hypoeutectic alloy has an overall composition below the eutectic composition on the stated solute scale, on the left side of that point.
“A Pb–Sn alloy at 50 wt% Sn is hypoeutectic and forms primary α before its remaining liquid freezes.”
Hypoeutectoid steel
A hypoeutectoid steel has less than the eutectoid carbon content and can form proeutectoid ferrite before the remaining austenite transforms.
“A 0.40 wt% C hypoeutectoid steel develops ferrite first and then pearlite during slow cooling.”

I

Incongruent transformation
An incongruent transformation changes the composition of at least one phase, as in a eutectic, eutectoid or peritectic reaction.
“Incongruent transformation on heating can leave a new solid together with liquid instead of melting to one same-composition liquid.”
Intermediate solid solution
An intermediate solid solution is a single solid phase stable over a composition range that does not extend to either pure component.
“In copper–zinc, β is an intermediate solid solution, while the copper-rich α phase is terminal.”
Intermetallic compound
An intermetallic compound is an ordered compound with a definite chemical formula and usually a very narrow composition range.
“Fe₃C is an intermetallic compound whose formula gives a carbon content near 6.70 wt% on the iron–carbon phase diagram.”
Invariant reaction
An invariant reaction is a fixed-temperature equilibrium reaction involving three phases in a binary system at constant pressure.
“An invariant reaction appears as a horizontal line because its three phase compositions and temperature are fixed.”
Iron–graphite diagram
The iron–graphite diagram describes equilibrium with graphite as the carbon-rich phase, in contrast to the metastable iron–cementite map.
“The iron–graphite diagram supplies the appropriate phase endpoints when cast iron separates carbon as graphite.”
Isomorphous system
An isomorphous system is a binary system whose components dissolve completely in each other in both liquid and solid states.
“Copper–nickel is an isomorphous system with a single FCC solid solution across its composition range.”

L

Lamellae
Lamellae are thin layers arranged side by side, such as the alternating solid phases that grow together in a eutectic or pearlitic structure.
“Short diffusion distances between lamellae help supply the different compositions needed by neighboring layers.”
Ledeburite
Ledeburite is the eutectic microconstituent initially formed as austenite plus cementite from 4.30 wt% C liquid at 1147 °C.
“A 3.0 wt% C carbide-forming iron develops primary austenite and about 40% ledeburite at the eutectic.”
Lever rule
The lever rule calculates phase fractions from the relative tie-line distances required to conserve total mass and component mass.
“Using the opposite tie-line arm in the lever rule gives the α mass fraction of a partly frozen alloy.”
Liquidus
The liquidus is the boundary above which an alloy is entirely liquid and below which solid begins to coexist with liquid.
“During slow cooling of an alloy, the first solid appears when its vertical path crosses the liquidus.”

M

Mass fraction
A mass fraction is the mass of a selected phase or constituent divided by the total sample mass, expressed between zero and one.
“A 2 kg sample with 0.5 kg solid has a solid mass fraction of 0.25, regardless of the solid’s composition.”
Metastable state
A metastable state persists for a long time despite a lower-energy state being available, because the change toward it is very slow.
“Cementite can remain in a metastable state in steel even though iron and graphite are more stable.”
Microconstituent
A microconstituent is a recognizable structural part of a material that can contain one phase or a distinctive mixture of phases.
“Pearlite is a microconstituent whose alternating layers contain both ferrite and cementite.”
Microconstituent fraction
A microconstituent fraction measures how much of the whole sample belongs to a recognizable structure, which may contain several phases.
“The eutectic microconstituent fraction includes both α and β formed from the last liquid to freeze.”
Microstructure
A microstructure is the observable combination of phases, their amounts, and their size, shape and arrangement within a material.
“A polished steel section reveals a microstructure of ferrite grains and darker pearlite colonies.”

O

Overall composition
The overall composition is the component concentration averaged over the entire alloy, including every phase that the alloy contains.
“In a partly frozen 35 wt% Ni alloy, the overall composition stays at 35 wt% Ni while its solid and liquid phases have different nickel contents.”

P

Pearlite
Pearlite is a microconstituent of alternating ferrite and cementite layers formed by the eutectoid transformation of austenite.
“Pearlite occupies all of a slowly cooled eutectoid steel, yet still contains two distinct solid phases.”
Pearlite colony
A pearlite colony is a region of pearlite in which ferrite and cementite layers share a common local growth arrangement.
“A pearlite colony can grow inward from a former austenite grain boundary as carbon redistributes.”
Peritectic reaction
A peritectic reaction is an invariant transformation in which liquid and one solid react to form a different solid during cooling.
“The iron–carbon peritectic reaction combines liquid and δ-ferrite to form γ-austenite at 1493 °C.”
Phase
A phase is a homogeneous region of matter with uniform physical and chemical characteristics and a boundary separating it from other phases.
“Ice and liquid water are different phases even though both contain only the water component.”
Phase field
A phase field is a region of a phase diagram labeled with the phase or phases stable over that range of conditions.
“A point inside the α + L phase field identifies coexisting solid solution and liquid at that location.”
Primary phase
A primary phase is a solid phase that forms from liquid before the remaining liquid undergoes a eutectic reaction during cooling.
“The primary phase in a 50 wt% Sn alloy is α, which forms before the remaining liquid becomes eutectic.”
Proeutectoid cementite
Proeutectoid cementite is cementite formed from austenite above A1 in a hypereutectoid steel, before the eutectoid reaction.
“Proeutectoid cementite is only part of total cementite because pearlite supplies additional carbide layers.”
Proeutectoid ferrite
Proeutectoid ferrite is ferrite formed from austenite above the eutectoid temperature, before the remaining austenite becomes pearlite.
“Proeutectoid ferrite accounts for about 49% of a slowly cooled 0.40 wt% C steel near A1.”

S

Solid solution
A solid solution is a single crystalline phase in which solute atoms replace host atoms or occupy gaps while the host structure remains.
“Nickel atoms occupy copper lattice sites in the FCC solid solution found in a Cu–Ni alloy.”
Solid-solution strengthening
Solid-solution strengthening is the increase in strength caused by dissolved solute atoms making dislocation movement more difficult.
“Solid-solution strengthening raises Cu–Ni strength even though the alloy can remain entirely one α phase.”
Solidus
The solidus is the boundary below which an alloy is entirely solid and above which liquid coexists with one or more solids.
“On heating a uniform Cu–Ni alloy, its first liquid appears as the temperature reaches the solidus.”
Solubility limit
The solubility limit is the largest concentration of a solute that can remain dissolved in a solvent at a particular temperature.
“Cooling a saturated alloy can cross its solubility limit and cause an additional solid phase to form.”
Solvus
A solvus is the boundary between a single solid-solution field and a field containing that solution together with another solid phase.
“Crossing the α solvus during cooling allows β particles to form in an already solid Pb–Sn alloy.”

T

Terminal solid solution
A terminal solid solution is a solid-solution phase whose composition field reaches one of the pure-component ends of a binary diagram.
“Lead-rich α is a terminal solid solution because its field extends to the pure-lead side of Pb–Sn.”
Tie line
A tie line is a horizontal segment across a two-phase field whose endpoints give the compositions of the phases at that temperature.
“At 1250 °C, the Cu–Ni tie line connects liquid at 31.5 wt% Ni with α at 42.5 wt% Ni.”
Triple point
A triple point is the temperature and pressure at which three phases of a one-component substance coexist in equilibrium.
“At water’s triple point, ice, liquid water and vapor coexist near 0.01 °C and 611.657 Pa.”

V

Volume fraction
A volume fraction is the volume occupied by a selected phase or constituent divided by the total volume of the sample.
“A dense phase can have a volume fraction smaller than its mass fraction because it occupies less space.”

W

Weight percent
Weight percent expresses a component’s mass as a percentage of the total mixture mass, commonly abbreviated wt%.
“An alloy at 30 weight percent nickel contains 30 g of nickel in every 100 g of the whole alloy.”

About this lesson

By StudeliReport a mistake

Make your own Study Materials

Turn your notes, slides and documents into Study Guides, Practice Questions, Flashcards and 6 more tools.

Get Started