Imperfections and Diffusion

Real crystals are never perfect, and their defects control much of how materials behave. Learn to identify vacancies, interstitials, solute atoms, dislocations and grain boundaries, estimate how many vacancies a metal holds, and measure grain size from a micrograph. Then follow atoms as they move through solids: explain the vacancy and interstitial mechanisms, calculate steady-state flux with Fick's first law, solve carburizing and doping problems with Fick's second law, and predict how strongly temperature speeds diffusion.

BeginnerLesson 3 of 9 in Materials Science and Engineering Course

What you will learn

  1. Recognize the defects that involve single atomic sites, estimate how many vacancies a metal holds at a given temperature, explain when one element dissolves in another, and express alloy compositions in the forms that diffusion calculations need.
    • Explain vacancies and self-interstitials and calculate how many there are
      Classify crystal defects by dimension, describe vacancies and self-interstitials, and use the equilibrium vacancy equation with correct units and absolute temperature.
    • Describe impurities and substitutional and interstitial solid solutions
      Distinguish solvent and solute, substitutional and interstitial solid solutions, apply the Hume-Rothery rules, and explain why carbon dissolves so differently in FCC and BCC iron.
    • Convert alloy compositions between weight percent, atom percent and kilograms per cubic meter
      Express the composition of a two-element alloy in weight percent, atom percent and mass per unit volume, and choose the form each calculation needs.
  2. Describe the line and planar defects that give metals their structure at the scale of grains, characterize dislocations by their Burgers vector, and measure grain size from a micrograph with standard methods.
    • Describe edge, screw and mixed dislocations and their Burgers vectors
      Picture edge, screw and mixed dislocations, determine and calculate Burgers vectors, use dislocation density, and connect dislocation motion with plastic deformation.
    • Explain surfaces, grain boundaries and other interfacial and bulk defects
      Describe external surfaces, grain boundaries, twin boundaries, stacking faults and phase boundaries, explain why interfaces carry energy, and recognize bulk defects and atomic vibrations.
    • Observe microstructure and measure grain size
      Explain how microstructures are prepared and observed, and determine grain size with the ASTM grain size number, the metric ISO index and the intercept method.
  3. Explain how and why atoms move through a solid by vacancy and interstitial jumps, and use Fick's first law to calculate the flux through a plate under steady-state conditions.
    • Explain the atomic mechanisms of diffusion
      Describe interdiffusion and self-diffusion, the conditions for an atomic jump, and the vacancy and interstitial mechanisms, using the Kirkendall effect as evidence.
    • Calculate steady-state diffusion with Fick's first law
      Define diffusion flux and concentration gradient, apply Fick's first law with consistent SI units, and solve for flux, diffusion coefficient or thickness under steady-state conditions.
  4. Use the error-function solution of Fick's second law to predict concentration profiles, and design surface treatments by finding the times, depths and temperatures they require.
    • Use the error-function solution to find concentrations
      State Fick's second law, apply its solution for a semi-infinite solid with constant surface concentration, read error-function values, and check when the solution is valid.
    • Find times, depths and temperatures for diffusion treatments
      Rearrange the error-function solution to find treatment times and depths, use the constant-Dt rule and the diffusion length for quick estimates, and describe dopant diffusion in semiconductors.
  5. Calculate how strongly temperature speeds diffusion, find activation energies from measured data, and compare diffusion rates across diffusing species, crystal structures and diffusion paths.
    • Calculate diffusion coefficients with the Arrhenius equation
      Use the Arrhenius form of the diffusion coefficient with tabulated data, absolute temperature and consistent units, and judge how sensitive diffusion is to temperature.
    • Find activation energies and temperatures from diffusion data
      Determine the activation energy and pre-exponential factor from an Arrhenius plot or two measurements, and use them to predict a diffusion coefficient or the temperature that a process needs.
    • Compare diffusion rates across species, crystal structures and paths
      Explain how the diffusing species, the host crystal structure, bonding and fast paths such as grain boundaries affect diffusion rates, and use these factors to reason about real processes.

Imperfections and Diffusion study guide

5 chapters

1

Point defects and alloy composition

Point defects change which atomic sites are occupied, and solute atoms change which elements occupy them. Those small differences affect how many jumps atoms can make and how much of an element a crystal can hold. Start by counting vacancies and identifying solid solutions, then express alloy composition on a mass, atom or volume basis. Keeping these quantities distinct makes the later diffusion equations easier to use.

1.1 Empty sites and extra atoms

A real crystal contains small disruptions in its regular atomic pattern. Their dimensions help you describe them: vacancies and interstitials are point defects, dislocations are line defects, boundaries are interfacial defects, and pores, cracks and inclusions are volume defects. These features affect strength, electrical conductivity, corrosion and diffusion.

Two kinds of point defect

A vacancy is an empty site that would normally hold an atom. A self-interstitial is an extra host atom squeezed into a void between normal sites. The extra atom pushes strongly against its neighbors, so its formation energy is much higher. Metals contain far fewer self-interstitials than vacancies.

Vacancies exist at equilibrium above 0 K. Making one costs energy, but spreading a small number of vacancies among many possible sites increases entropy. The balance between these effects gives a stable, nonzero vacancy fraction.

Calculate a vacancy population

The introductory equilibrium equation is

Nv=Nexp⁡(−QvkT).

Here, Nv and N are numbers per unit volume, Qv is the energy to form one vacancy, and T is in kelvins. Use k=8.62×10−5 eV/K when the energy is in eV per atom. For energy in J per atom, use 1.38×10−23 J/K. A molar formation energy instead requires R=8.314 J/(mol·K). The exponential is the fraction of sites that are empty; it must lie between 0 and 1. This equation omits a formation-entropy prefactor and gives an order-of-magnitude estimate.

Find the site density from density and atomic weight:

N=NAρA.

For aluminum, use NA=6.022×1023 atoms/mol, ρ=2.70 g/cm³ and A=26.98 g/mol. The result is 6.03×1022 atoms/cm³, or 6.03×1028 atoms/m³. One cubic meter contains one million cubic centimeters, so the number per cubic meter is larger by that factor.

At 600 °C, T=873 K. With Qv=0.67 eV,

QvkT=0.67(8.62×10−5)(873)=8.90.

Thus the fraction is e−8.90=1.36×10−4 and the vacancy density is about 8.2×1024 m⁻³. That is roughly one vacant site per 7400 sites. Using 600 in the exponent gives a much smaller, incorrect result: the temperature scale must start at absolute zero.

At 300 K, the same estimate gives a fraction of 5.6×10−12. The strong temperature dependence helps explain why atoms move much more readily through a hot metal. Quenching can trap an excess vacancy population because the vacancies cannot all disappear during rapid cooling.

Charged crystals

Ionic solids must keep electrical neutrality. In NaCl, a Schottky pair consists of one missing sodium ion and one missing chloride ion. In AgCl, a Frenkel pair forms when a silver ion leaves its regular site for an interstitial site. Both examples preserve the overall cation-to-anion ratio. The Frenkel pair contains a displaced ion; the Schottky pair contains two vacancies.

Key Takeaways

  • Point, line, interfacial and volume defects describe different spatial scales.
  • Self-interstitials strongly strain the lattice and are rare in metals.
  • Use absolute temperature and matching energy units in the vacancy equation.
  • Convert site density to the volume unit required by the answer.
  • Vacancies increase sharply with temperature and enable lattice-atom jumps.
  • Ionic defect combinations preserve electrical neutrality.

1.2 How solute atoms fit into a crystal

An alloy contains elements added to a metal to change its properties. Foreign atoms are not always unwanted: adding copper to silver, for example, makes sterling silver harder and more resistant to wear. Even a metal described as highly pure still contains many impurity atoms in a macroscopic piece.

The solvent is the main component and the solute is the smaller component. A homogeneous solid solution has solute spread through one crystal structure. Once the solubility limit is exceeded, a second phase appears. One crystal structure containing two atom types is different from two separate kinds of crystal.

Where the solute sits
SolutionSolute positionExample
SubstitutionalReplaces a host atom on a regular siteNickel in copper
InterstitialOccupies a void between host atomsCarbon in iron

Hydrogen, carbon, nitrogen and oxygen are small enough to form interstitial solutions in suitable hosts. Even these atoms distort the lattice. Their dissolved concentrations are usually low, commonly below about 10%.

Predict substitutional solubility

The Hume-Rothery rules identify conditions favorable to extensive substitutional solution:

  1. Atomic radii differ by less than about 15% relative to the solvent radius.
  2. The elements have the same crystal structure.
  3. Their electronegativities are similar; a large difference favors compounds.
  4. With other factors equal, a metal tends to dissolve more of a higher-valence metal than of a lower-valence one.

For nickel in copper,

rNi−rCurCu×100%=0.125−0.1280.128×100%=−2.3%.

The small mismatch, shared FCC structure and similar electronegativity support the extensive Cu–Ni solid solution. The rules are empirical guidelines: meeting them makes complete solubility possible but does not guarantee it. Silver and copper have only a 12.5% radius difference and share FCC structure, yet their mutual solid solubility is limited. Zinc has an HCP structure, so complete substitutional solubility in FCC copper is unfavorable, although alpha brass can contain about 35 wt% zinc.

Why carbon fits better in FCC iron

Packing factor measures the total fraction of space occupied by atoms. Solubility also depends on the size and shape of individual interstitial sites.

Host structureOctahedral site radiusTetrahedral site radius
FCC0.414 times the host radius0.225 times the host radius
BCC0.155 times the host radius0.291 times the host radius

For an iron atom radius near 0.124 nm, the largest geometrical void is about 0.051 nm in FCC and 0.036 nm in BCC. Carbon, with a radius near 0.071 nm, strains either lattice. FCC iron nevertheless accommodates much more carbon: austenite reaches about 2.1 wt% at 1147 °C, while ferrite reaches only about 0.022 wt% at 727 °C.

BCC has a lower packing factor, but its empty space is divided into smaller sites. More empty space in total does not mean a larger site for a particular atom. The amount that dissolves and the speed at which it moves are also different properties: interstitial carbon can move rapidly through ferrite despite its low solubility.

Key Takeaways

  • Substitutional atoms occupy regular sites; interstitial atoms occupy voids.
  • A homogeneous solid solution is a single phase with a shared crystal structure.
  • The Hume-Rothery rules guide predictions but do not guarantee complete solubility.
  • Individual site size explains carbon solubility better than total empty space.
  • Austenite holds much more carbon than ferrite.

1.3 Convert the basis of an alloy composition

A composition must say what is being counted. Weight percent, also called mass percent, compares masses. Atom percent compares numbers of atoms, or equivalently moles. Diffusion flux calculations often need a third quantity: the mass of solute in each cubic meter of alloy.

Start with a convenient sample

For a two-element alloy,

C1=m1m1+m2×100,C1′=n1n1+n2×100.

Moles follow from n=m/A, with the mass and atomic weight in compatible units. In either percentage system the two components add to 100, but a weight percentage and an atom percentage cannot be added together.

A 100 g sample makes weight-percent calculations easy. For brass with 70 wt% Cu and 30 wt% Zn, take 70 g copper and 30 g zinc. Convert each mass to moles:

nCu=70/63.55=1.1015,nZn=30/65.38=0.4589.

The zinc fraction of the total moles is about 0.294, so the composition is 29.4 at% zinc and 70.6 at% copper. Copper and zinc have similar atomic weights, so the two percentage scales give similar values.

The direct binary conversion is

C1′=C1A2C1A2+C2A1×100.

The other element's atomic weight appears beside each weight percentage because this form comes from multiplying both parts of the mole ratio by both atomic weights. Working with a 100 g sample avoids having to memorize that arrangement.

Convert atom percent back to weight percent

Start with a total of 100 mol of atoms. Multiply each component's mole amount by its atomic weight and divide by total mass:

C1=C1′A1C1′A1+C2′A2×100.

For 50 at% nickel and 50 at% copper, the masses are proportional to 58.69 and 63.55. Nickel supplies 58.69/(58.69+63.55)×100=48.0 wt%. Equal atom counts do not give equal masses when the atomic weights differ. In steel the difference is larger: 0.80 wt% carbon corresponds to about 3.6 at% because each carbon atom is much lighter than each iron atom.

Find mass per alloy volume

Using additive component volumes, a binary alloy gives

C1′′=C1C1/ρ1+C2/ρ2×103.

Insert weight percentages as numbers and pure-component densities in g/cm³; the answer is kg/m³. For 0.80 wt% carbon steel, with graphite density 2.25 g/cm³ and iron density 7.87 g/cm³,

CC′′=0.800.80/2.25+99.2/7.87×103=61.7 kg/m3.

This is an estimate because the component volumes are assumed to add. The factor of 1000 converts g/cm³ to kg/m³.

For Fick's first law, concentration in kg/m³ leads to mass flux in kg/(m²·s). In the error-function concentration ratio, the concentration units cancel. All three concentrations may use wt% provided they use the same basis. Changing only one concentration to at% would destroy that consistency.

Key Takeaways

  • Weight percent uses masses; atom percent uses moles or atom counts.
  • Convert mass to moles by dividing by atomic weight.
  • For the reverse conversion, multiply mole amounts by atomic weights.
  • Mass per volume is the concentration needed for SI mass flux.
2

Dislocations, interfaces and grain size

A metal can look uniform while containing many differently oriented crystals and long lines of atomic misalignment. Dislocations explain how local slips change shape; boundaries show where one crystal meets another. Connect these atomic pictures with micrographs, then measure grain size from counts or test lines. The measurement method and magnification determine how an image becomes a physical length or area count.

2.1 Dislocation lines and the Burgers vector

A dislocation is a line of lattice misalignment. Atoms close to the line are displaced; farther away the crystal is nearly regular. Dislocations form during solidification and can multiply during plastic deformation. Thermal stresses during cooling can also create them.

Edge, screw and mixed character
TypeAtomic pictureBurgers vector relative to line
EdgeThe end of an extra half-planePerpendicular
ScrewPlanes form a spiral rampParallel
MixedBoth edge and screw characterAn intermediate angle

For an edge dislocation, the extra half-plane crowds atoms on its side of the line, creating compression. Atoms on the opposite side are stretched in tension. The edge of the half-plane is the line defect; the entire half-plane is not the dislocation line. A screw dislocation can be pictured as two regions shifted by shear so that the planes form a continuous ramp around the line.

Measure the lattice displacement

A Burgers circuit takes equal atom-to-atom steps around a region. The steps close in a perfect lattice. Around a dislocation they leave a closure failure. With a consistent circuit convention, the vector that closes the circuit is the Burgers vector, 𝐛. Its length and direction describe the slip displacement associated with the defect.

A curved dislocation can be screw at one point and edge at another. Its Burgers vector stays the same along the line; the local line direction changes. Classifying the entire curved line from just one local angle would miss this mixed character.

For common metal dislocations, the vector follows a close-packed direction:

  • FCC: 𝐛=(a/2)⟨110⟩, giving magnitude a2/2.
  • BCC: 𝐛=(a/2)⟨111⟩, giving magnitude a3/2.
  • Common HCP basal slip: the magnitude is a.

For copper, a=0.3615 nm gives b=0.256 nm. For BCC iron, a=0.2866 nm gives b=0.248 nm. The direction indices determine the length factor; the lattice parameter alone is not the Burgers-vector length in FCC or BCC.

How much line is present?

Dislocation density is total dislocation length divided by specimen volume. Its unit is m/m³, or m⁻². A well-annealed metal may have about 1010 m⁻², while a heavily cold-worked metal can reach 1015 m⁻² or more. At 1014 m⁻², a volume of 1 cm³ contains 1014×10−6=108 m of line. A count of lines crossing a section needs an orientation correction before it represents length per volume.

Why metals can change shape

A moving dislocation breaks and remakes bonds locally, one row at a time. This needs much less stress than sliding a whole atomic plane at once. Pushing a wrinkle along a rug gives a useful picture of this localized motion. When the dislocation crosses a crystal, it leaves a relative slip displacement equal to its Burgers vector. The visible surface-step height is the component normal to the surface, not always the full vector length. Strong ionic and covalent bonding makes this motion harder in ceramics.

Transmission electron microscopy can show individual dislocations. Suitable etching can reveal pits where dislocation lines meet a polished surface.

Key Takeaways

  • The dislocation is a line of misalignment, not a row of vacancies.
  • The Burgers vector is perpendicular to an edge line and parallel to a screw line.
  • A curved dislocation keeps its Burgers vector while its local character changes.
  • Dislocation density measures line length per volume.
  • Slip proceeds by local bond rearrangement along a moving dislocation.

2.2 Surfaces, grain boundaries and larger defects

An interfacial defect extends across an area. It usually separates regions with different lattice orientations or structures. External surfaces are included because the ordered crystal ends there. At an external surface, atoms have fewer bonded neighbors and therefore higher energy than atoms inside.

Energy at a boundary

Surface and interfacial energies are measured per area, in J/m². Reducing area lowers the total excess energy when the energy per area is fixed. This explains the tendency of an unconstrained liquid drop to become spherical. It also helps explain why grains grow during heating: larger grains leave less boundary area per specimen volume.

A polycrystalline metal contains many crystalline grains. Across a grain boundary, the orientation changes through a region only a few atomic distances wide. Atoms remain bonded across the boundary. A grain boundary is not a crack, and a collection of crystalline grains is not an amorphous solid.

Boundaries are less regularly packed than grain interiors. They often etch faster, collect impurity atoms and provide faster diffusion paths. High-angle boundaries generally have greater energy than small-angle boundaries; special ordered boundaries can have relatively low energies.

Small orientation differences

A small-angle tilt boundary can be modeled as a wall of edge dislocations. For Burgers-vector magnitude b and dislocation spacing h,

θ≈bh,

where the angle is in radians. With b=0.256 nm and h=10 nm, the angle is 0.0256 rad. Multiplying by 180/π gives about 1.5°. Reducing the spacing increases the misorientation. A small-angle twist boundary is described by an arrangement of screw dislocations.

Interfaces with special relationships
InterfaceWhat changes across it?
Grain boundaryCrystal orientation
Twin boundaryOrientation changes by a specific mirror relationship
Phase boundaryStructure, composition or both change between phases
Stacking faultThe regular order of close-packed planes is interrupted

In a twin, one lattice mirrors the other across the twin plane. Mechanical twins form under shear, especially in BCC and HCP metals. Annealing twins appear during heat treatment, commonly in FCC copper and brass. Their good atomic fit helps give twin boundaries low energy.

FCC planes normally stack in the sequence ABCABCABC. A stacking fault can introduce a short region with an ABAB sequence, like the local order in HCP. The letters label positions of whole planes; a stacking fault is a planar defect, not an isolated missing atom.

Volume defects and thermal motion

Pores, cracks and inclusions occupy three-dimensional regions. Examples include shrinkage pores left by solidification and slag particles trapped in steel. Regions of a second phase can also be treated as volume features; their surrounding interfaces are phase boundaries.

Atoms vibrate around their sites, typically about 1013 times per second. The amplitude grows with temperature. These vibrations supply the energy for occasional diffusion jumps. A vibration is motion around a site; a diffusion jump changes which site an atom occupies.

Key Takeaways

  • Interfaces carry excess energy per area.
  • Atoms remain bonded across grain boundaries.
  • Small-angle tilt boundaries can be represented by edge-dislocation arrays.
  • Twin boundaries have a mirror relationship; phase boundaries separate phases.
  • Stacking faults disrupt the order of close-packed planes.
  • Pores, cracks and inclusions are volume defects.

2.3 Read micrographs and measure grain size

Microstructure describes the size, shape and arrangement of features such as grains and phases. A polished metal surface often needs etching before its grains become visible. Grinding removes roughness, polishing produces a mirror finish, and etching reveals differences in orientation and boundary reactivity.

Grains with different orientations etch and reflect light differently. Boundaries etch into shallow grooves that scatter light away from the objective, so they look dark. The dark network is therefore evidence of boundary relief, not an open network of cracks.

Choose a useful microscope
MethodTypical information
Optical microscopyGrain and phase patterns; resolution about 0.2 µm
SEMSurface detail with a large depth of field
TEMThin-foil detail, including individual dislocations
Scanning probe microscopySurface topography, potentially at atomic scale

Magnification enlarges an image; resolution determines whether nearby features can be distinguished. Enlarging an optical image cannot reveal details below its resolution limit.

Count grains per area

The ASTM E112 grain size number is defined by

N100=2G−1,

where N100 is the average grain count per square inch of a 100× image. The area unit is part of this definition. A larger G means finer grains: increasing it by 1 doubles the grain count in a fixed specimen area.

At another magnification M, first convert the image-area count:

N100=NM(M100)2.

For 45 grains per square inch at 250×, the corrected count is 45(2.5)2=281.25. Then G=1+log⁡2(281.25)=9.1. The correction is squared because both image dimensions change. A fixed image area at high magnification shows a smaller specimen area; scaling its count to 100× increases the count.

For a standard area count, count grains fully inside the region and use half counts for grains crossing its edge. Count several representative regions so that one unusually coarse or fine patch does not dominate the estimate.

The ISO 643 metric index for steels uses

m=8×2G,

with m in grains per mm² of actual specimen area. ISO G=7 gives 1024 grains/mm². ASTM G=7 corresponds to about 992 grains/mm². The scales nearly coincide but are not numerically identical.

Measure line intercepts

Draw test lines with total image length LT and count their grain-boundary intersections P. Divide by magnification to recover the specimen length:

ℓˉ=LTPM.

If the image lines total 500 mm, the magnification is 100× and there are 72 crossings, then ℓˉ=0.0694 mm, about 69 µm. This length estimates grain size along the test directions. The ASTM conversion is

G=−6.644log⁡10ℓˉ−3.288,

using the intercept length in millimeters. The example gives about 4.4. Magnification enters line lengths once and area counts twice. Mixing those two corrections can change the inferred grain size substantially.

Key Takeaways

  • Polishing and etching reveal grain structure in optical microscopy.
  • Resolution limits distinguishable detail, even at high magnification.
  • A larger grain size number means smaller grains.
  • Correct image-area counts with the square of the magnification ratio.
  • Correct intercept lengths with one magnification factor.
  • ASTM and ISO grain size numbers nearly coincide but use different definitions.
  • Finer grains provide more boundary area per volume.
3

Atomic jumps and steady diffusion

Atoms can move through a solid while the solid keeps its overall shape. Follow the empty sites and interstitial spaces that make jumps possible, then distinguish the random motion of individual atoms from a measurable net flow. A concentration profile links that motion to an engineering calculation: the amount passing through each square meter of a plate each second. Signs, thickness and concentration units give that result its meaning.

3.1 How random jumps transport atoms

Diffusion transports matter through atomic motion. Join copper and nickel and heat them below their melting points: each element spreads into the other, creating a region whose composition changes smoothly with position. This is interdiffusion. Atoms also move in a pure metal without changing its composition; this is self-diffusion, measured using tracer isotopes.

Two requirements for a jump

An atom needs an empty neighboring destination and enough thermal energy to pass the barrier between sites. Its neighbors must move apart temporarily, bonds must change, and the lattice distorts during the jump. Heating increases the fraction of atoms able to cross that energy barrier.

The individual jumps are random. A region rich in a species sends more atoms across an imaginary dividing plane than a region containing fewer of that species. The imbalance gives a net flow down the concentration gradient. When concentration becomes uniform, the opposing jump rates balance. Atomic motion continues even though the net flux is zero.

Vacancy and interstitial routes
MechanismMoving atom and destinationMain rate limitation
Vacancy diffusionA lattice atom enters an adjacent empty lattice siteBoth vacancies and jump energy are needed
Interstitial diffusionA small atom moves between interstitial sitesA free interstitial site and jump energy are needed

In vacancy diffusion, an atom moves one way while the vacancy effectively moves the other way. This is the main route for host atoms and substitutional solutes in metals. Vacancies become much more abundant as temperature rises, adding to the temperature effect on jump frequency.

Hydrogen, carbon, nitrogen and oxygen can move through interstitial sites in suitable metals. Almost all neighboring interstitial destinations are empty in a dilute solution, so a small solute does not have to wait for a rare lattice vacancy. Interstitial diffusion is usually much faster than substitutional diffusion.

Evidence from unequal atomic flows

The Kirkendall effect shows that the two species need not cross a diffusion couple at equal rates. In the classic brass–copper experiment, molybdenum marker wires were placed on a brass core before it was coated with copper. After heating at 785 °C, zinc had moved out of the brass faster than copper moved in. The core shrank and the markers moved closer together.

A mechanism in which atoms only exchange directly in pairs would force equal opposing atomic transfers. Vacancy-mediated movement allows unequal species flows, balanced by a vacancy counterflow. Where atoms leave faster than they arrive, vacancies may accumulate into Kirkendall voids. Marker motion tracks the lattice's displacement, not simply the diffusion distance of one species.

Processing uses

Carburizing supplies carbon to a steel surface; nitriding supplies nitrogen. Doping introduces small controlled amounts of elements into silicon. Diffusion bonding joins contacting solids through atomic transport. Diffusion can also be unwanted: steel can lose carbon from its surface during heating in an atmosphere with a low carbon potential. All of these processes depend on atoms moving through solids, even though that movement is much slower than diffusion in many gases and liquids.

Key Takeaways

  • Atomic jumps need an empty destination and enough energy.
  • A concentration gradient biases net flow without directing each individual jump.
  • Vacancy diffusion moves atoms and vacancies in opposite directions.
  • Interstitial diffusion is usually faster because small atoms have many empty destinations.
  • Self-diffusion leaves overall composition unchanged.
  • Kirkendall marker motion reveals unequal species fluxes and vacancy transport.

3.2 Calculate transport through a steady plate

Diffusion flux is the amount crossing each unit area per unit time. If mass M crosses area A during time t at constant flux,

J=MAt.

A mass flux has units kg/(m²·s). An atomic flux instead counts atoms/(m²·s). Flux is not the total amount transported: a larger sheet carries more mass at the same flux because it has more area.

Read the concentration profile

A concentration profile plots concentration against position. Its slope is the concentration gradient, dC/dx. In steady state the profile does not change with time. A plate held at fixed face concentrations has a linear steady profile when the diffusion coefficient is constant.

With face A at xA and face B at xB, the gradient is

dCdx=CB−CAxB−xA.

State the positive position direction before assigning a flux sign. Fick's first law gives

J=−DdCdx.

The coefficient D, or diffusivity, has units m²/s. If concentration falls as position increases, the gradient is negative and the flux is positive. The minus sign expresses transport down the concentration gradient.

Work a plate calculation

An iron plate is 2.0 mm thick. At 700 °C, take D=2.2×10−11 m²/s and carbon face concentrations of 0.60 and 0.10 kg/m³. Choose positive position from the richer face toward the poorer face.

  1. Convert the thickness: 2.0 mm=2.0×10−3 m.
  2. Find the gradient: (0.10−0.60)/(2.0×10−3)=−250 kg/m⁴.
  3. Multiply by the negative diffusivity: J=−(2.2×10−11)(−250)=5.5×10−9 kg/(m²·s).

For a 1 m² plate in 3600 s, the mass is M=JAt=2.0×10−5 kg, about 20 mg. Leaving thickness in millimeters would make the calculated flux 1000 times too small. If the concentrations were supplied as wt%, they would first need conversion to mass per volume for this mass-flux result.

Solve for another unknown

Using magnitudes, D=JΔx/ΔC. A flux of 1.2×10−8 kg/(m²·s), thickness 5.0 mm and concentration difference 3.0 kg/m³ give

D=(1.2×10−8)(5.0×10−3)3.0=2.0×10−11 m2/s.

At fixed face concentrations and temperature, halving thickness doubles the gradient and flux. Doubling the area doubles total mass flow while leaving flux unchanged. These are distinct ways to increase production through a membrane, such as a palladium sheet used to separate hydrogen.

Know what the model describes

Fick's first law relates local flux to the local gradient, including during nonsteady diffusion. A changing profile also requires conservation of mass and Fick's second law to predict its later shape. A curved steady profile can occur if diffusivity depends on composition. In some alloys chemical interactions even allow uphill concentration transport: chemical potential is the more general driving quantity. The constant-coefficient concentration model describes dilute-solution estimates.

Key Takeaways

  • Flux measures amount per area per time.
  • A constant-D steady plate has a linear concentration profile.
  • The flux sign follows the chosen position axis.
  • Convert lengths to meters before combining them with SI diffusivity.
  • At fixed concentrations, a thinner plate carries a larger flux.
4

Concentration profiles and treatment design

Surface treatments build a concentration profile that changes with time. The useful question may be how much solute reaches a depth, how long a target takes, or how changing temperature alters that time. The error-function solution connects these questions for a maintained surface concentration. Its initial and boundary conditions matter as much as the algebra, especially when comparing a steel surface treatment with a fixed-dose dopant drive-in.

4.1 Calculate a changing concentration profile

In nonsteady diffusion, concentration changes with time at each location. The flux entering a small region can differ from the flux leaving it. The difference accumulates there. Combining this mass balance with Fick's first law gives, for constant diffusivity,

∂C∂t=D∂2C∂x2.

Positive upward curvature means concentration is increasing locally. A slope sets flux; curvature sets how that flux changes from one position to the next.

Match the surface conditions

A useful solution describes a solid initially uniform at C0. From the start of treatment, one surface stays at Cs. The solid is semi-infinite when its far side stays effectively unaffected. For constant D,

Cx−C0Cs−C0=1−erf⁡(x2Dt).

Define z=x/(2Dt). The error function is

erf⁡(z)=2π∫0ze−y2 dy.

It starts at 0 and tends toward 1. The concentration ratio therefore equals 1 at the surface and tends toward 0 far inside. These limits are useful checks on the subtraction order.

Look up the error function
zerf(z)zerf(z)
0.10.11250.60.6039
0.20.22270.70.6778
0.30.32860.80.7421
0.40.42840.90.7969
0.450.47551.00.8427
0.50.52051.20.9103
1.50.96612.00.9953

Interpolate between nearby entries or use a calculator's error-function command. The required concentration ratio is one minus the table value, not the table value itself.

Add carbon to steel

Take C0=0.20 wt%, Cs=1.00 wt%, D=1.1×10−11 m²/s and t=2.5×104 s. At a depth of 1.0 mm,

Dt=5.24×10−4 m,z=0.954.

The error function is about 0.822, so

Cx=0.20+(1.00−0.20)(1−0.822)=0.34 wt%.

The result lies between the initial and surface values and approaches the initial value at greater depth.

Remove carbon from steel

The same solution covers decarburization. With initial carbon 0.80 wt%, surface carbon 0.10 wt%, D=5.9×10−12 m²/s, 3600 s and a depth of 0.20 mm, the argument is 0.686. Since its error function is about 0.668,

Cx=0.80+(0.10−0.80)(1−0.668)=0.57 wt%.

The negative surface-minus-initial difference produces a decrease. Do not swap the concentrations to force this difference positive.

All concentrations must share a basis; wt% works because units cancel. Use meters and seconds with diffusivity in m²/s. Check uniform initial composition, fixed surface composition and constant diffusivity. As a practical semi-infinite check, the part thickness should exceed about 10Dt. A thin sheet approaching uniform saturation needs different boundary conditions.

Key Takeaways

  • Fick’s second law describes concentration accumulation from unequal local fluxes.
  • The error-function solution requires uniform initial and fixed surface concentrations.
  • Use the complement of erf for the concentration ratio.
  • The same signed expression covers both enrichment and depletion.
  • Check units and whether the far surface remains unaffected.

4.2 Choose a treatment time or depth

A target concentration identifies a position on a diffusion profile. Once the initial and surface values are fixed, the same target always has the same error-function argument. This lets you calculate a time, a depth or a trade between time and temperature.

Find the argument first

Form the concentration ratio and then its complement:

r=Cx−C0Cs−C0,erf⁡(z)=1−r.

Read the argument z from a table or inverse error function. The geometry of the solution then gives

t=x24z2D,x=2zDt.

For steel starting at 0.20 wt% carbon with its surface at 1.00 wt%, a target of 0.60 wt% gives r=0.50. The required error-function value is also 0.50. Interpolating between 0.4755 at an argument of 0.45 and 0.5205 at 0.50 gives z≈0.477.

At 950 °C, take D=1.1×10−11 m²/s. To reach the target at 0.50 mm,

t=(5.0×10−4)24(0.477)2(1.1×10−11)≈2.5×104 s.

This is about 6.9 h. Squaring a depth expressed in millimeters while using SI diffusivity would give a million-fold error in time.

Scale the same target

For fixed initial and surface concentrations, x2/(Dt) stays constant for a chosen target. At fixed temperature, depth grows with the square root of time. Doubling the target depth requires four times the time; tripling time increases the depth by a factor of 3.

The diffusion length, Dt, measures the characteristic spread. It is not a sharp front: concentration changes smoothly beyond it. The halfway concentration occurs at about 0.95Dt in this fixed-surface solution.

For the same whole profile at a different constant temperature,

D1t1=D2t2.

If the diffusivity increases from 1.1×10−11 to 1.95×10−11 m²/s, a 6.9 h treatment shortens to about 3.9 h. Check the far-side condition after calculating the result: the first treatment has 10Dt≈5.2 mm.

Distinguish the two doping stages

In silicon predeposition, the surface receives a continuing supply of dopant and its concentration is held constant. The error-function profile applies. During drive-in, the external supply is removed and a fixed dose per area spreads deeper. The surface concentration then falls.

When the original deposited layer is shallow compared with the drive-in diffusion length, a thin-source approximation gives

C(x,t)=Q0πDtexp⁡(−x24Dt).

Here Q0 is dose per unit area, so dividing by a length gives concentration per volume. The approximation needs the thin initial layer as well as a fixed dose. A junction depth is where the introduced dopant concentration equals the opposite-type background concentration.

Key Takeaways

  • Find the error-function argument before solving for time or depth.
  • At a fixed target composition, depth squared is proportional to Dt.
  • Matching Dt reproduces the same fixed-surface profile.
  • The diffusion length describes a spread, not a sharp penetration front.
  • Predeposition fixes surface concentration; drive-in redistributes a fixed dose.
  • A Gaussian drive-in profile assumes a sufficiently shallow initial layer.
5

Temperature and material effects

A diffusion coefficient only becomes useful when its temperature, moving species and host are known. The Arrhenius relation connects temperature to the energy barrier for atomic motion, and measured data let you recover that barrier. Use the fitted parameters to predict processing conditions, then compare the roles of crystal structure and fast paths. A material can hold little solute yet allow that solute to move quickly.

5.1 Calculate diffusivity at a temperature

The diffusivity is not a fixed property independent of processing conditions. Heating both raises the frequency of successful jumps and, for vacancy diffusion, increases the vacancy population. The Arrhenius equation combines these effects in a useful temperature relation:

D=D0exp⁡(−QdRT).

The pre-exponential factor D0 has units m²/s. The activation energy Qd is in J/mol, and R=8.314 J/(mol·K). Temperature is absolute: use T=temperature in °C+273. For activation energies per atom, use a matching Boltzmann constant instead of the molar gas constant.

Interpret the energy barrier

Activation energy describes the barrier for diffusion. For equilibrium vacancy diffusion it includes vacancy formation and atom migration. Interstitial diffusion does not need a lattice vacancy, which helps explain its lower activation energy. With the same prefactor and temperature, a larger barrier makes diffusivity smaller. It also makes the coefficient more sensitive to a given change in reciprocal temperature.

Diffusing atom and hostD₀ in m²/sQ in kJ/mol
C in BCC iron1.1 × 10⁻⁶87.4
C in FCC iron2.3 × 10⁻⁵148
Fe in BCC iron2.8 × 10⁻⁴251
Fe in FCC iron5.0 × 10⁻⁵284
Cu in Cu7.8 × 10⁻⁵211

A row describes a particular species in a particular host structure. Do not take the prefactor from one row and the activation energy from another.

Work through the exponent

For carbon in FCC iron at 950 °C, use 1223 K and convert 148 kJ/mol to 148000 J/mol. Then

QdRT=1480008.314(1223)=14.56.

The exponential is about 4.77×10−7. Multiplying by the prefactor gives

D=(2.3×10−5)(4.77×10−7)=1.1×10−11 m2/s.

The exponent is dimensionless and negative. The result is smaller than the prefactor. Entering 148 with the gas constant in joules makes the barrier almost disappear; entering 950 instead of 1223 makes diffusion appear far too slow. If a prefactor is tabulated in cm²/s, multiply by 10−4 to express it in m²/s.

Recognize exponential sensitivity

Copper self-diffusivity rises from about 3.7×10−16 m²/s at 700 °C to 3.1×10−14 m²/s at 900 °C, roughly an 84-fold increase. Equal temperature increments do not produce equal additions to diffusivity.

Taking logarithms gives

ln⁡D=ln⁡D0−QdR1T.

Thus a plot of natural logarithm against reciprocal absolute temperature is linear. On a base-10 plot, the slope instead contains a factor of approximately 2.303 in the denominator. Moving right on either reciprocal-temperature plot means cooling, so the line slopes downward.

Key Takeaways

  • Match the species and host when choosing Arrhenius parameters.
  • Use kelvins and energy units compatible with the constant.
  • Activation energy controls the temperature sensitivity.
  • The Arrhenius plot is linear against reciprocal absolute temperature.

5.2 Infer activation energy and treatment temperature

Measurements at several temperatures let you fit the Arrhenius relationship. The fitted line reveals an activation energy and prefactor. Those parameters then predict a diffusivity or the temperature needed for a chosen process time.

Use a straight-line plot

For a vertical axis of ln⁡D and a horizontal axis of 1/T,

slope=−Qd/R,intercept=ln⁡D0.

For a vertical axis of log⁡10D, multiply the negative slope by 2.303R to get activation energy. Read the horizontal scale carefully. A graph against 1000/T compresses the slope magnitude by a factor of 1000 relative to the slope against 1/T. Choose points on the fitted line so individual measurement scatter does not dominate the estimate.

Fit two measurements

Eliminating the prefactor between two temperatures gives

Qd=Rln⁡(D2/D1)1/T1−1/T2.

For copper self-diffusion, take D1=3.7×10−16 m²/s at 973 K and D2=3.1×10−14 m²/s at 1173 K. The diffusivity ratio is about 83.8 and its natural logarithm is 4.428. The reciprocal-temperature difference is 1.752×10−4 K⁻¹. These give

Qd=8.314(4.428)1.752×10−4=2.10×105 J/mol.

The positive result fits the fact that diffusion speeds up on heating. Reversing only the temperature subtraction would produce an erroneous negative barrier.

Recover the prefactor by substituting either measurement:

D0=D2exp⁡(QdRT2).

Using the rounded fitted energy gives about 7.0×10−5 m²/s. At 1073 K, these rounded parameters predict about 4.2×10−15 m²/s. It lies between the measured coefficients, as expected. Carry unrounded fitted values through a calculation when you need more precision.

Find a temperature for a process target

Rearranging the same equation gives

T=QdRln⁡(D0/D).

First determine the coefficient the process needs. To reproduce a 6.9 h carburizing profile in 4.0 h, starting from D1=1.1×10−11 m²/s,

D2=D16.94.0=1.9×10−11 m2/s.

For carbon in FCC iron, insert D0=2.3×10−5 m²/s and Qd=148000 J/mol. The required temperature is about 1271 K, or 998 °C. The result is hotter than the original 950 °C, consistent with the shorter time.

Keep the fitted mechanism in view

A fit is most reliable within its measurement range and while the same host structure and diffusion mechanism apply. At lower temperatures, grain-boundary transport can become dominant and change the slope. A single straight-line extrapolation across such a change would combine different processes into one apparent activation energy.

Key Takeaways

  • An ln plot and a base-10 plot require different slope factors.
  • Check for a 1000/T axis before interpreting a slope.
  • Two coefficients and absolute temperatures determine an activation energy.
  • Find the required diffusivity before solving for a treatment temperature.
  • A mechanism change can invalidate a distant extrapolation.

5.3 Compare how atoms move through different materials

Diffusivity belongs to a species–host pair and a transport path. A value for carbon in iron cannot stand in for iron moving through iron. Crystal structure, bonding and the amount of boundary area also matter.

Compare species in one host

At 1000 °C in FCC iron, carbon has a diffusivity near 1.95×10−11 m²/s, while iron self-diffusivity is about 1.11×10−16 m²/s. Carbon moves roughly 175000 times faster. It is a small interstitial solute with many empty neighboring sites and a lower activation energy. Iron atoms move through vacancies, so their motion includes the cost of vacancy formation.

Separate solubility from mobility

At 900 °C, carbon diffusivity is about 1.4×10−10 m²/s in BCC ferrite and 5.9×10−12 m²/s in FCC austenite. BCC's more open migration paths give faster motion. Yet ferrite holds much less dissolved carbon than austenite.

QuestionRelevant property
How much carbon can remain dissolved?Solubility
How quickly does carbon redistribute?Diffusivity

Carburizing uses austenite, typically around 850–950 °C, because it can hold the needed carbon content. Choosing a phase solely for the largest diffusivity would miss that requirement. The larger useful FCC sites favor carbon storage, while BCC migration barriers favor speed; these are different parts of the atomic environment.

Compare bonding and temperature scale

Strong bonding tends to make atomic jumps harder and raise self-diffusion activation energy. At the same absolute temperature, high-melting metals generally diffuse more slowly. For many close-packed metals, the barrier is about 18RTm, with melting temperature in kelvins. Copper gives a ratio Qd/(RTm) near 18.7. Diffusion often becomes important above roughly 0.4 of the absolute melting temperature, though the relevant time and distance still matter.

Fast paths do not always carry most mass

Surfaces, grain boundaries and dislocation cores disrupt regular packing. Atoms often move faster along them than through a perfect grain interior. A typical ordering is

Dsurface>Dboundary>Dlattice.

The total transport also depends on how much cross-sectional area each path occupies. Coarse grains at high temperature can carry most mass through their interiors even though each boundary is a faster path. Fine grains provide more boundary area per volume. At lower temperature, lower-barrier paths become relatively more important, so a polycrystal's Arrhenius plot can bend to a shallower slope.

Other hosts and variable composition

Ions in ceramics often move by vacancies. Because moving ions carry charge, cation and anion transport is coupled by the requirement to keep the material neutral. In polymers, small molecules pass through spaces between chains; this allows oxygen or carbon dioxide to pass slowly through a container wall.

Diffusivity can change with composition. Carbon can move faster in austenite with higher carbon content. A constant coefficient is an approximation for a limited concentration interval; wider intervals may require an average or a composition-dependent model. Any comparison should keep species, host phase, temperature and path attached to its quoted coefficient.

Key Takeaways

  • Diffusivity depends on both the moving species and its host.
  • High solubility and fast diffusion are different properties.
  • Fast paths have lower migration barriers but occupy limited area.
  • Fine grains and lower temperatures can favor boundary transport.
  • Ceramic and polymer diffusion have different microscopic routes.

Imperfections and Diffusion examples

5 Walkthroughs

1

Count defects and describe alloy composition

15 steps
Move from lattice sites to vacancy numbers, solid solutions and useful concentration units.
  1. 1
    IntroductionStart with the occupied sites

    A crystal can contain empty sites, extra host atoms and foreign atoms. First decide which site is involved, then choose what to count. You will estimate a vacancy population, compare the ways solutes fit into a lattice and convert composition from a mass basis to an atom or volume basis. Each calculation starts by identifying the quantity the answer needs.

  2. 2
    ExplanationSort defects by their dimensions

    A point defect involves atomic sites, such as a vacancy or self-interstitial. A dislocation is a line defect; a grain boundary is an interfacial defect. A pore, crack or inclusion is a volume defect.

    A vacancy is an empty normal site. A self-interstitial is a host atom in a void. It strains its surroundings strongly, so metals contain far fewer self-interstitials than vacancies.

  3. 3
    ExplanationTemperature sets the vacancy fraction

    The equilibrium estimate is Nv/N=e−Qv/(kT). Formation costs energy, while a small vacancy population increases entropy. Their balance leaves some vacancies above 0 K.

    Use kelvins, and match the energy unit to the constant. For a formation energy in eV per atom, use k=8.62×10−5 eV/K. The exponential gives a fraction; it still needs multiplication by the site density to give vacancies per volume.

  4. 4
    ExampleFirst find the aluminum site density

    For aluminum, take density 2.70 g/cm³ and atomic weight 26.98 g/mol. Dividing density by atomic weight gives moles per cubic centimeter; multiplying by Avogadro’s number gives sites.

    N=(6.022×1023)(2.70)26.98=6.03×1022 cm−3.

    Multiply by one million to express the result per cubic meter: 6.03×1028 m⁻³.

  5. 5
    ExampleThen multiply by the empty-site fraction

    At 600 °C, aluminum is at 873 K. With formation energy 0.67 eV per atom, the exponent has magnitude 0.67/[(8.62×10−5)(873)]=8.90.

    Nv=(6.03×1028)e−8.90≈8.2×1024 m−3.

    The fraction, about 0.000136, is much smaller than one even though the number of vacancies in a macroscopic volume is enormous.

  6. 6
    ChallengeApply the fraction to a new metal

    A metal has 5.0×1028 sites/m³ and an equilibrium vacancy fraction of 4.0×10−6. How many vacancies are in 2.0 mm³?

    ---reveal---

    First find the vacancy density: Nv=(5.0×1028)(4.0×10−6)=2.0×1023 m⁻³. The volume is 2.0×10−9 m³, so it contains 4.0×1014 vacancies. The fraction, density and total count are three different quantities.

  7. 7
    ConnectionPreserve charge in ionic defects

    In NaCl, removing one sodium ion and one chloride ion creates a Schottky pair. In AgCl, moving a silver ion from its normal site into a void creates a Frenkel pair.

    Both keep overall electrical neutrality. The first example has two empty sites; the second has one empty site and one displaced ion. A self-interstitial in a pure metal and an interstitial ion are related site pictures in different materials.

  8. 8
    ExplanationLocate a dissolved foreign atom

    A substitutional solute replaces a host atom. An interstitial solute occupies a void between regular sites. Nickel in copper illustrates the first; carbon in iron illustrates the second.

    A homogeneous solid solution keeps one crystal structure with mixed atoms. The solvent is the main component. Adding more solute than the solubility limit allows produces a second phase.

  9. 9
    ExampleUse the solubility guidelines

    Nickel and copper have radii 0.125 and 0.128 nm. Relative to copper, the mismatch is (0.125−0.128)/0.128×100%=−2.3%. Both are FCC and have similar electronegativity.

    Small size mismatch, shared structure, similar electronegativity and favorable valence support extensive substitutional solution. These Hume-Rothery guidelines fit the Cu–Ni example but do not guarantee complete solubility for every pair.

  10. 10
    Key InsightLook at individual voids

    BCC iron has a lower packing factor than FCC iron, yet its useful interstitial sites are smaller. Empty volume spread among many small sites cannot hold the same solute as fewer larger sites.

    Austenite can hold much more carbon than ferrite. Carbon still strains either lattice because it is larger than the unstrained void. Solubility depends on accommodation in the sites; diffusion speed concerns the barriers between them.

  11. 11
    ChallengeJudge a proposed alloy

    A host has radius 0.160 nm and an FCC structure. A proposed solute has radius 0.184 nm and an HCP structure. What do these two observations suggest about complete substitutional solubility?

    ---reveal---

    The size mismatch is 0.024/0.160=15%, near the approximate size limit. The structures also differ, so complete substitutional solubility is unfavorable. Limited solution can still occur; the guidelines do not require zero solubility.

  12. 12
    ExampleTurn mass into atom counts

    For brass containing 70 wt% copper and 30 wt% zinc, choose a 100 g sample. Divide the component masses by 63.55 and 65.38 g/mol.

    nCu=1.1015 mol,nZn=0.4589 mol.

    Zinc contributes 0.4589/(1.1015+0.4589)×100=29.4 at%. Using moles avoids comparing the masses as though copper and zinc atoms had identical weights.

  13. 13
    ExplanationChoose mass per volume for flux

    A mass flux in kg/(m²·s) needs concentration in kg/m³. For a binary alloy, estimate component volumes by dividing each component mass by its pure-element density, then sum those volumes.

    For 0.80 g carbon and 99.2 g iron, the volumes are approximately 0.80/2.25+99.2/7.87=12.96 cm³. Carbon mass divided by this volume gives 0.0617 g/cm³, or 61.7 kg/m³. This estimate assumes additive volumes.

  14. 14
    ChallengeConvert a composition for a transport calculation

    A binary alloy contains equal numbers of X and Y atoms. Their atomic weights are 20 and 60 g/mol. Both pure densities are 4.0 g/cm³, and volumes add. What is the mass concentration of X?

    ---reveal---

    Equal mole amounts have masses in the ratio 20:60, so X is 25 wt%. Equal component densities give alloy density 4000 kg/m³. Thus X contributes 0.25(4000)=1000 kg/m³. A substitutional or interstitial label alone would not supply this concentration.

  15. 15
    RecapKeep the counting basis visible

    Identify the site first: an empty regular site is a vacancy, a host atom in a void is a self-interstitial, and solute atoms can occupy either regular sites or voids.

    For calculations, distinguish vacancy fraction, vacancy density and total count. For alloys, distinguish mass share, atom share and mass per volume. The basis and units determine which quantity can enter the next equation.

2

Follow a lattice defect into a micrograph

15 steps
Connect dislocation geometry, boundary energy and magnification-corrected grain measurements.

Save this lesson to follow every Walkthrough step by step.

  1. 1
    IntroductionConnect atomic geometry with visible structure
  2. 2
    ExplanationUse the line direction to classify a dislocation
  3. 3
    ExampleCalculate a Burgers-vector length
  4. 4
    ChallengeInterpret a curved line
  5. 5
    ExampleMeasure how much line is present
  6. 6
    AnalogyMove a wrinkle through the lattice
  7. 7
    ExplanationRecognize a bonded boundary
  8. 8
    ConnectionDistinguish special interfaces
  9. 9
    ExampleEstimate a small-angle boundary
  10. 10
    ChallengePredict the effect of dislocation spacing
  11. 11
    ExplanationPrepare the feature before measuring it
  12. 12
    ExampleCorrect an area count
  13. 13
    ExampleCorrect a line measurement
  14. 14
    ChallengeUse a grain count to infer available paths
  15. 15
    RecapMatch the geometry to the measurement
3

Build a flux calculation from atomic jumps

12 steps
Explain random motion, identify the jump mechanism and calculate steady transport through a plate.

Save this lesson to follow every Walkthrough step by step.

  1. 1
    IntroductionFrom individual jumps to a measurable flow
  2. 2
    ExplanationIdentify the two jump requirements
  3. 3
    AnalogyExplain the direction of the net flow
  4. 4
    ConnectionRead the evidence from markers
  5. 5
    ChallengeInterpret continued tracer spreading
  6. 6
    ExplanationDefine flux before calculating an amount
  7. 7
    ExampleFind the steady gradient
  8. 8
    ExampleTurn the slope into flux and mass
  9. 9
    Key InsightPredict a thickness change
  10. 10
    ChallengeCalculate a new membrane flux
  11. 11
    ChallengeSeparate motion from accumulation
  12. 12
    RecapUse the profile and the units together
4

Work with the error-function profile

15 steps
Calculate a concentration, invert the solution for time and check the surface and thickness conditions.

Save this lesson to follow every Walkthrough step by step.

  1. 1
    IntroductionDecide what the surface supplies
  2. 2
    ExplanationConnect accumulation to curvature
  3. 3
    ExplanationChoose the fixed-surface solution
  4. 4
    ExampleCalculate the length scale
  5. 5
    ExampleRecover the local concentration
  6. 6
    ChallengeApply the profile during depletion
  7. 7
    TipCheck whether the far side matters
  8. 8
    ExampleConvert a target into an argument
  9. 9
    ExampleSolve for the time
  10. 10
    ChallengeScale a target depth
  11. 11
    ConnectionTrade diffusivity against duration
  12. 12
    ExplanationDistinguish fixed concentration from fixed dose
  13. 13
    ChallengeFind a changed process requirement
  14. 14
    Key InsightLocate a semiconductor junction
  15. 15
    RecapCheck the profile before trusting the number
5

Fit temperature dependence and compare diffusion paths

14 steps
Use Arrhenius calculations, interpret slopes and connect effective transport with species and path area.

Save this lesson to follow every Walkthrough step by step.

  1. 1
    IntroductionAttach a coefficient to its conditions
  2. 2
    ExplanationMatch the units in Arrhenius
  3. 3
    ExampleCalculate carbon diffusivity
  4. 4
    ChallengeDiagnose an oversized coefficient
  5. 5
    ExplanationRead the slope on the right axes
  6. 6
    ExampleInfer an energy from two measurements
  7. 7
    ExampleRecover a coefficient or temperature
  8. 8
    ChallengeInterpret a fitted graph
  9. 9
    Key InsightKeep storage and speed separate
  10. 10
    ExplanationInclude how much area a fast path has
  11. 11
    ChallengeExplain a change in the Arrhenius line
  12. 12
    ConnectionRecognize other material routes
  13. 13
    ChallengeCombine a time target with a barrier
  14. 14
    RecapRead a diffusion number with its full meaning

Imperfections and Diffusion practice questions

50 Practice Questions in 5 sets

Set 1: Atomic defects and grain measurements10 Practice Questions

Question 1 of 10

A micrograph at 150× has 450 mm of test lines and 60 grain-boundary crossings. Using the mean-intercept relation and G = −6.644 log₁₀ ℓ̄ − 3.288 with ℓ̄ in mm, what ASTM grain size number results?
  1. 3.36
  2. 7.36
  3. 5.36
  4. −9.09
Show answerHide answer
Answer: C
The specimen intercept length is 450/(60×150)=0.050 mm. Inserting that millimeter value gives G=−6.644log⁡10(0.050)−3.288=5.36. Converting to 50 µm and then inserting 50 into a formula calibrated for millimeters produces an invalid negative result.

Question 2 of 10

A host atom occupies a void between regular sites in a pure metal. What defect is present?
  1. A substitutional solute
  2. A self-interstitial
  3. A lattice vacancy
  4. An interstitial solute
Show answerHide answer
Answer: B
A self-interstitial is a host atom forced into a space between normal lattice sites. An interstitial solute also occupies a void, but it is a foreign element; the question specifies that the atom belongs to the pure host metal.

Question 3 of 10

A metal has 6.0×1028 sites/m³, a vacancy formation energy of 0.75 eV and a temperature of 1000 K. Using k=8.62×10−5 eV/K, what is the equilibrium vacancy density?
  1. 1.7×10−4 m⁻³
  2. 3.5×1032 m⁻³
  3. 1.0×1025 m⁻³
  4. 5.2×1027 m⁻³
Show answerHide answer
Answer: C
The vacancy fraction is e−0.75/(8.62×10−5×1000)≈1.66×10−4. Multiplying by the site density gives about 1.0×1025 vacancies/m³. Reporting the exponential alone confuses a dimensionless fraction with a number per volume.

Question 4 of 10

Where are zinc atoms located in a substitutional copper-rich solid solution?
  1. On regular sites replacing copper atoms
  2. In voids between regular copper sites
  3. On sites only at external surfaces
  4. In separate crystals of pure zinc
Show answerHide answer
Answer: A
A substitutional solute takes a regular lattice site that could otherwise hold a host atom. The shared crystal structure is retained. Placement between regular sites describes an interstitial solution, which requires a different fit between the solute and host atoms.

Question 5 of 10

An FCC host has radius 0.140 nm. An FCC solute has radius 0.154 nm and similar electronegativity. What conclusion follows from these data?
  1. The 10% mismatch rules out a substitutional solution entirely
  2. The 9.1% mismatch guarantees a completely miscible solution
  3. The 9.1% mismatch requires an interstitial solid solution
  4. The 10% mismatch favors, but does not ensure, extensive solution
Show answerHide answer
Answer: D
The radius mismatch relative to the host is (0.154−0.140)/0.140=0.10, or 10%. It meets the approximate size guideline, and the shared structure also favors solution. These empirical conditions do not guarantee complete solubility; the host radius, not the solute radius, is the denominator.

Question 6 of 10

An alloy contains 20 wt% element X and 80 wt% element Y. Their atomic weights are 40 and 80 g/mol. What is the atom percent of X?
  1. 20.0 at%
  2. 11.1 at%
  3. 50.0 at%
  4. 33.3 at%
Show answerHide answer
Answer: D
For a 100 g sample, X contributes 20/40=0.50 mol and Y contributes 80/80=1.00 mol. X is therefore one third of the total atoms, or 33.3 at%. Keeping the value at 20% would treat unequal atomic weights as though they were equal.

Question 7 of 10

A dislocation’s Burgers vector is parallel to its local line direction. What is its local character?
  1. Pure edge
  2. Pure screw
  3. Mixed edge and screw
  4. A wall of edge dislocations
Show answerHide answer
Answer: B
Pure screw character occurs where the Burgers vector and dislocation line are parallel. Pure edge character requires a perpendicular relationship. A curved line can show different local characters without changing its Burgers vector, so the question concerns the specified location.

Question 8 of 10

An FCC metal has lattice parameter 0.420 nm. What Burgers-vector magnitude corresponds to common perfect-dislocation slip?
  1. 0.297 nm
  2. 0.210 nm
  3. 0.364 nm
  4. 0.594 nm
Show answerHide answer
Answer: A
For common FCC slip, the magnitude is a2/2. Substituting 0.420 nm gives 0.297 nm. The nearby value 0.364 nm comes from the BCC factor 3/2, so the crystal structure determines which geometric factor applies.

Question 9 of 10

What atomic relationship identifies a twin boundary?
  1. The lattices have an arbitrary angle across a plane
  2. One lattice ends at a free external surface
  3. The lattices are mirror-related across a plane
  4. Two phases share only the same chemical composition
Show answerHide answer
Answer: C
A twin boundary has a specific mirror relationship between the lattices on its two sides. A general grain boundary may join arbitrarily misoriented grains, so misorientation alone is insufficient. The mirror arrangement also allows a relatively good atomic fit and low boundary energy.

Question 10 of 10

A square region on a 200× micrograph has area 2.0 in². It contains 56 complete grains and 16 grains crossing the border. What is its ASTM grain size number?
  1. 6.0
  2. 8.0
  3. 7.0
  4. 8.2
Show answerHide answer
Answer: B
The effective count is 56+16/2=64 grains, giving 32 per in² of image. Correcting to 100× gives 32(200/100)2=128, so G=1+log⁡2128=8. Counting every border grain as whole gives a larger result, while omitting magnification gives 6.
Set 2: From atomic jumps to concentration profiles10 Practice Questions

Save this lesson to see every answer and practice every set.

Question 1 of 10

A pure metal has uniform composition at a high temperature. What does zero net self-diffusion flux mean?
  1. Atoms have stopped jumping between sites
  2. No vacancies remain anywhere in the crystal
  3. Opposing atomic jumps balance on average
  4. All atoms exchange in permanently fixed pairs
Show answerHide answer

Save this lesson to see this answer.

Question 2 of 10

In a diffusion couple, species A crosses the original interface faster than species B crosses in the reverse direction. Why can lattice markers move?
  1. Unequal atom flows are accompanied by vacancy transport
  2. Atoms swap directly one-for-one across the interface
  3. The faster species shifts from lattice to interstitial sites
  4. Markers move only when both intrinsic fluxes are equal
Show answerHide answer

Save this lesson to see this answer.

Question 3 of 10

A steady membrane has D=3.0×10−10 m²/s and thickness 1.5 mm. Concentration falls from 1.8 to 0.6 kg/m³ along the positive x direction. What is the mass flux?
  1. −2.4×10−7 kg/(m²·s)
  2. +2.4×10−10 kg/(m²·s)
  3. +3.6×10−10 kg/(m²·s)
  4. +2.4×10−7 kg/(m²·s)
Show answerHide answer

Save this lesson to see this answer.

Question 4 of 10

A membrane carries a constant flux of 4.0×10−8 kg/(m²·s) through 0.25 m² for 2.0 h. What mass crosses it?
  1. 2.0×10−8 kg
  2. 7.2×10−5 kg
  3. 2.9×10−4 kg
  4. 1.8×10−5 kg
Show answerHide answer

Save this lesson to see this answer.

Question 5 of 10

For a maintained surface concentration in the semi-infinite error-function solution, what is the ratio (Cₓ − C₀)/(Cₛ − C₀) at the surface?
  1. 1
  2. 0
  3. 0.5
  4. −1
Show answerHide answer

Save this lesson to see this answer.

Question 6 of 10

A solid starts at 0.30 wt% solute and its surface is held at 1.10 wt%. At a particular depth and time, erf(z) = 0.60. What is the concentration there?
  1. 0.78 wt%
  2. 0.44 wt%
  3. 0.62 wt%
  4. 0.96 wt%
Show answerHide answer

Save this lesson to see this answer.

Question 7 of 10

A target composition reaches 0.40 mm depth after 3.0 h. At the same temperature and with unchanged initial and surface concentrations, how long does it take to reach 0.80 mm?
  1. 6 h
  2. 1.5 h
  3. 24 h
  4. 12 h
Show answerHide answer

Save this lesson to see this answer.

Question 8 of 10

Which temperature enters the Arrhenius equation for a treatment at 827 °C?
  1. 827 K
  2. 1100 K
  3. 554 K
  4. 1373 K
Show answerHide answer

Save this lesson to see this answer.

Question 9 of 10

A treatment takes 5.0 h to reach a target at 0.60 mm with D1=8.0×10−12 m²/s. A new treatment uses D2=2.0×10−11 m²/s. With the same initial, surface and target compositions, how long is needed at 0.90 mm?
  1. 4.5 h
  2. 2.0 h
  3. 3.0 h
  4. 11.25 h
Show answerHide answer

Save this lesson to see this answer.

Question 10 of 10

A process has D0=1.0×10−4 m²/s and Q=160 kJ/mol. Its current coefficient is 1.0×10−12 m²/s. What temperature will reproduce the same fixed-surface profile in half the time? Use R=8.314 J/(mol·K).
  1. About 772 °C
  2. About 1086 °C
  3. About 919 °C
  4. About 813 °C
Show answerHide answer

Save this lesson to see this answer.

Set 3: Connect composition, defects and measurement10 Practice Questions

Save this lesson to see every answer and practice every set.

Question 1 of 10

A silver ion in AgCl leaves a lattice site and occupies a nearby interstitial site. What defect combination is created?
  1. A paired-cation-vacancy Schottky defect
  2. Two vacancies of opposite ionic charge
  3. A substitutional solute and host vacancy
  4. A vacancy–interstitial Frenkel pair
Show answerHide answer

Save this lesson to see this answer.

Question 2 of 10

Why is a low atomic packing factor insufficient to predict high interstitial solubility?
  1. The host with more empty volume must always have larger individual sites
  2. The available empty volume may be divided into small individual sites
  3. Packing factor measures the solute’s migration barrier at each temperature
  4. Packing factor fixes the chemical identity of atoms that can replace the host
Show answerHide answer

Save this lesson to see this answer.

Question 3 of 10

A binary alloy is 40 at% X and 60 at% Y. Atomic weights are 50 and 100 g/mol, and pure-element densities are 5.0 and 10.0 g/cm³. Under additive volumes, what is the mass concentration of X?
  1. 2500 kg/m³
  2. 4000 kg/m³
  3. 2000 kg/m³
  4. 3125 kg/m³
Show answerHide answer

Save this lesson to see this answer.

Question 4 of 10

A density of dislocation lines is quoted in m⁻². What length divided by what quantity does it represent?
  1. Total dislocation length divided by surface area
  2. Number of vacancies divided by specimen volume
  3. Total dislocation length divided by specimen volume
  4. Number of grains divided by image area
Show answerHide answer

Save this lesson to see this answer.

Question 5 of 10

A specimen has dislocation density 3.0×1013 m⁻² and volume 2.0 mm³. What total line length does it contain?
  1. 6.0×1010 m
  2. 6.0×107 m
  3. 6.0×104 m
  4. 1.5×1022 m
Show answerHide answer

Save this lesson to see this answer.

Question 6 of 10

A small-angle tilt boundary has unchanged Burgers-vector magnitude but twice the dislocation spacing. How does its angle change?
  1. It increases to twice its previous value
  2. It decreases to half its previous value
  3. It remains equal to its previous value
  4. It decreases to one quarter of its value
Show answerHide answer

Save this lesson to see this answer.

Question 7 of 10

An ISO grain size index of 5 is measured in steel. Approximately how many grains would lie in a 2000 mm² image area at 200×? Treat it as an area-average estimate.
  1. 12.8 grains
  2. 512000 grains
  3. 2560 grains
  4. 128 grains
Show answerHide answer

Save this lesson to see this answer.

Question 8 of 10

An alloying element is observed to substitute on regular host sites. What main diffusion route is expected in the metal?
  1. Jumps only between empty interstitial voids
  2. Migration only within external surface layers
  3. Direct equal-rate exchanges of different atom pairs
  4. Jumps into neighboring lattice vacancies
Show answerHide answer

Save this lesson to see this answer.

Question 9 of 10

Two polycrystals have identical chemistry and grain-boundary width. One has much finer grains. At low temperature, its measured effective diffusivity is higher and its ln D versus 1/T line is shallower. What explanation fits both observations?
  1. More boundary area makes a higher-barrier path more important
  2. More boundary area makes a lower-barrier path more important
  3. Fewer boundaries make a lower-barrier lattice path more important
  4. Finer grains raise lattice activation energy while leaving paths unchanged
Show answerHide answer

Save this lesson to see this answer.

Question 10 of 10

A steady membrane must pass 1.8×10−4 kg in 2.0 h through 0.10 m². Its thickness is 0.80 mm and face concentrations differ by 2.0 kg/m³. What diffusivity is needed?
  1. 1.0×10−10 m²/s
  2. 2.5×10−7 m²/s
  3. 4.0×10−11 m²/s
  4. 1.0×10−7 m²/s
Show answerHide answer

Save this lesson to see this answer.

Set 4: Design and check diffusion treatments10 Practice Questions

Save this lesson to see every answer and practice every set.

Question 1 of 10

A solid starts at 0.90 wt% solute and its surface is held at 0.15 wt%. At a depth where erf(z) = 0.80, what is the solute concentration?
  1. 0.30 wt%
  2. 0.60 wt%
  3. 0.75 wt%
  4. 1.05 wt%
Show answerHide answer

Save this lesson to see this answer.

Question 2 of 10

During decarburization with a lower maintained surface concentration, where does the concentration approach its initial value in the semi-infinite model?
  1. Far inside the solid
  2. At the exposed surface
  3. At all depths at once
  4. Beyond a sharp front
Show answerHide answer

Save this lesson to see this answer.

Question 3 of 10

A thick solid starts at 0.10 wt% solute and has a surface held at 0.90 wt%. How long until 0.20 mm depth reaches 0.50 wt% when D=4.0×10−12 m²/s? Use erf(0.45) = 0.4755 and erf(0.50) = 0.5205.
  1. About 0.76 h
  2. About 6.10 h
  3. About 12.2 h
  4. About 3.05 h
Show answerHide answer

Save this lesson to see this answer.

Question 4 of 10

A plate is 0.40 mm thick. A proposed one-face treatment has D=1.0×10−11 m²/s and lasts 1.0 h. Using the practical thickness criterion, is the semi-infinite solution appropriate?
  1. Yes; the suggested thickness scale is about 0.19 mm
  2. No; the suggested thickness scale is about 1.90 mm
  3. No; the suggested thickness scale is about 0.019 mm
  4. Yes; the suggested thickness scale is about 0.019 mm
Show answerHide answer

Save this lesson to see this answer.

Question 5 of 10

A maintained-surface treatment takes 8.0 h with D=6.0×10−12 m²/s. What time gives the same profile at D=1.6×10−11 m²/s?
  1. 21.3 h
  2. 3.0 h
  3. 5.0 h
  4. 1.5 h
Show answerHide answer

Save this lesson to see this answer.

Question 6 of 10

A species has D0=4.0×10−5 m²/s and Q=120 kJ/mol. What is D at 927 °C? Use R=8.314 J/(mol·K).
  1. 6.92×10−12 m²/s
  2. 3.95×10−5 m²/s
  3. 2.39×10−6 m²/s
  4. 2.39×10−10 m²/s
Show answerHide answer

Save this lesson to see this answer.

Question 7 of 10

A species has D=2.0×10−15 m²/s at 900 K and D=2.0×10−13 m²/s at 1100 K. What is its fitted activation energy? Use R=8.314 J/(mol·K).
  1. 190 kJ/mol
  2. 82.3 kJ/mol
  3. −190 kJ/mol
  4. 0.190 kJ/mol
Show answerHide answer

Save this lesson to see this answer.

Question 8 of 10

A fitted log₁₀ D plot falls from −12.0 to −15.0 as the horizontal coordinate 1000/T rises from 0.80 to 1.00. What activation energy does the line imply? Use R = 8.314 J/(mol·K).
  1. 125 kJ/mol
  2. 0.287 kJ/mol
  3. 287 kJ/mol
  4. −287 kJ/mol
Show answerHide answer

Save this lesson to see this answer.

Question 9 of 10

A shallow dopant layer is driven in with fixed dose per area, constant D and a Gaussian thin-source profile. Its surface concentration is 4.0×1024 atoms/m³ after 1.0 h. What is the surface value after 4.0 h? Both times satisfy the thin-source approximation.
  1. 4.0×1024 atoms/m³
  2. 1.0×1024 atoms/m³
  3. 2.0×1024 atoms/m³
  4. 8.0×1024 atoms/m³
Show answerHide answer

Save this lesson to see this answer.

Question 10 of 10

In one phase at one temperature, solute A has DA=9DB. Both receive the same initial and maintained surface concentrations. How do their depths for the halfway concentration compare after equal times?
  1. A reaches three times the depth reached by B
  2. A reaches nine times the depth reached by B
  3. A reaches the same depth as B at equal times
  4. A reaches one third of the depth reached by B
Show answerHide answer

Save this lesson to see this answer.

Set 5: Combine structure, data and process decisions10 Practice Questions

Save this lesson to see every answer and practice every set.

Question 1 of 10

What property describes the maximum dissolved solute content of a phase under specified conditions?
  1. Diffusivity
  2. Solubility
  3. Dislocation density
  4. Surface energy
Show answerHide answer

Save this lesson to see this answer.

Question 2 of 10

A metal has density 8.0 g/cm³, atomic weight 64 g/mol and vacancy formation energy 0.90 eV. Estimate its equilibrium vacancies per m³ at 727 °C using NA=6.022×1023 mol⁻¹ and k=8.62×10−5 eV/K.
  1. 2.20×1018 m⁻³
  2. 4.36×1022 m⁻³
  3. 2.93×10−5 m⁻³
  4. 2.20×1024 m⁻³
Show answerHide answer

Save this lesson to see this answer.

Question 3 of 10

A binary alloy is 25 at% X and 75 at% Y, with atomic weights 20 and 60 g/mol. Their densities are both 5.0 g/cm³, and component volumes add. What is the mass concentration of X?
  1. 500 kg/m³
  2. 1250 kg/m³
  3. 250 kg/m³
  4. 1500 kg/m³
Show answerHide answer

Save this lesson to see this answer.

Question 4 of 10

A boundary is modeled as edge dislocations with b = 0.280 nm separated by 8.0 nm. What is its approximate misorientation in degrees?
  1. 0.035°
  2. 1.00°
  3. 2.01°
  4. 4.01°
Show answerHide answer

Save this lesson to see this answer.

Question 5 of 10

Two images of the same region contain 24 grains/in² at 300× and 54 grains/in² at 200×. What ASTM grain size number do these measurements support?
  1. About 8.75
  2. About 5.58
  3. About 6.75
  4. About 9.75
Show answerHide answer

Save this lesson to see this answer.

Question 6 of 10

A steady membrane originally delivers 1.0×10−4 kg in 1.0 h. A new membrane has half the thickness and three quarters of the area, with unchanged D and face concentrations. How long will it take to deliver 3.0×10−4 kg?
  1. 1.0 h
  2. 1.5 h
  3. 4.0 h
  4. 2.0 h
Show answerHide answer

Save this lesson to see this answer.

Question 7 of 10

During a fixed-surface treatment, C₀ = 0.25 wt% and Cₛ = 1.05 wt%. A depth must reach 0.45 wt%. What error-function value corresponds to this target?
  1. 0.25
  2. 0.50
  3. 0.75
  4. 0.80
Show answerHide answer

Save this lesson to see this answer.

Question 8 of 10

Two diffusion coefficients are 1.0×10−14 m²/s at 1000 K and 1.0×10−12 m²/s at 1200 K. Assuming one Arrhenius mechanism, what D is predicted at 1100 K?
  1. 1.00×10−13 m²/s
  2. 5.05×10−13 m²/s
  3. 8.11×10−14 m²/s
  4. 1.23×10−13 m²/s
Show answerHide answer

Save this lesson to see this answer.

Question 9 of 10

A silicon wafer’s dopant supply is removed after deposition. The deposited layer is still thick compared with the subsequent drive-in diffusion length. Is the thin-source Gaussian profile justified?
  1. Yes; removing the supply always creates an initially thin source
  2. No; fixed dose alone does not establish a thin initial source
  3. No; a fixed dose requires the constant-surface error-function profile
  4. Yes; every fixed dose has a maintained surface concentration
Show answerHide answer

Save this lesson to see this answer.

Question 10 of 10

Two parallel transport paths have effective area fractions 0.999 for lattice and 0.001 for boundaries. At the same imposed concentration gradient, D_boundary = 100 D_lattice. What fraction of total mass flux follows the boundary path?
  1. About 99.0%
  2. About 9.1%
  3. About 0.1%
  4. About 50.0%
Show answerHide answer

Save this lesson to see this answer.

Stuck on your own question? Homework Help

Key Terms

68 Key Terms, each with its definition

A

Activation energy
Activation energy for diffusion is the effective energy barrier for thermally activated atomic transport, often stated per mole.
Vacancy-mediated transport includes energy for vacancy formation as well as atom migration.
Additive-volume approximation
The additive-volume approximation estimates alloy volume by summing component masses divided by their pure-component densities.
A binary alloy’s weight percentages can be converted to kg/m³ using estimated component volumes.
Alloy
An alloy is a metallic material containing deliberately added elements that alter its properties, such as wear resistance.
Copper added to silver makes sterling silver harder than pure silver and more resistant to wear.
Arrhenius equation
The Arrhenius equation expresses diffusivity as a prefactor times an exponential containing a negative energy-to-thermal-energy ratio.
Carbon diffusivity in FCC iron rises sharply when the treatment temperature increases from 950 to 1000 °C.
Arrhenius plot
An Arrhenius plot graphs the logarithm of diffusivity against reciprocal absolute temperature to reveal a diffusion energy barrier.
A downward straight line on an ln plot yields activation energy from the negative slope times the gas constant.
ASTM grain size number
The ASTM grain size number relates average grain count to image area at 100×; a larger number means finer average grains.
At the reference magnification, raising the number by one doubles the count of grains per image area.
Atom percent
Atom percent is an element’s number of atoms, or moles of atoms, divided by the alloy total and multiplied by 100.
Equal atom percentages of nickel and copper give unequal weight percentages because their atoms differ in mass.

B

Burgers vector
The Burgers vector is the lattice displacement associated with a dislocation, found from a consistently defined circuit’s closure failure.
For common FCC slip, its magnitude is the lattice parameter multiplied by the square root of two and divided by two.

C

Concentration gradient
A concentration gradient is the rate at which concentration changes with position, giving the local slope of its profile.
A drop of 0.5 kg/m³ across 0.002 m produces a gradient magnitude of 250 kg/m⁴.

D

Diffusion
Diffusion is transport of matter by atomic or molecular movement, arising in solids through many individual thermally activated jumps.
Carbon introduced at a steel surface can spread into the interior while the steel remains solid.
Diffusion coefficient
The diffusion coefficient is the mobility parameter linking flux to concentration gradient, with units of square meters per second.
A coefficient must identify the moving species, host structure and temperature before it can be compared.
Diffusion flux
Diffusion flux is the amount of a species passing through a unit area perpendicular to transport in a unit of time.
A membrane with twice the area transports twice the mass at the same uniform flux and duration.
Diffusion length
Diffusion length is the characteristic distance given by the square root of diffusivity times time for a diffusion process.
At constant diffusivity, quadrupling treatment time doubles the characteristic spread of the profile.
Dislocation
A dislocation is a line defect around which atoms depart from their regular positions, allowing local slip as it moves.
Transmission electron microscopy can reveal the dislocation lines within a thin metal foil.
Dislocation density
Dislocation density is the total length of dislocation line per unit specimen volume, expressed as inverse square meters.
Multiplying a density of 10¹⁴ m⁻² by a volume of 10⁻⁶ m³ gives 10⁸ m of dislocation line.
Drive-in
Drive-in is the doping stage in which an already deposited, fixed dose spreads farther into silicon after its supply is removed.
A shallow initial dopant layer can be approximated by a Gaussian profile after sufficient drive-in.

E

Edge dislocation
An edge dislocation is the line where an extra half-plane ends inside a crystal; its Burgers vector is perpendicular to that line.
An extra half-plane compresses atoms on its side of the edge line and stretches them on the opposite side.
Equilibrium vacancy fraction
The equilibrium vacancy fraction is the share of lattice sites that are empty at a specified temperature after equilibration.
Multiplying a vacancy fraction by the site density gives the number of vacancies per cubic meter.
Error function
The error function is an integral-based function that rises from zero toward one and describes the fixed-surface diffusion profile.
The surface concentration ratio equals one minus the error-function value, so the complement matters.
Etching
Etching is the controlled chemical attack of a prepared surface that reveals differences in grain orientation and boundary reactivity.
After polishing, etching creates boundary grooves that scatter light and show up as dark lines.
Extrapolation
Extrapolation estimates a value beyond the measured range by extending a fitted relationship, which requires the mechanism to remain valid.
Extending a high-temperature lattice-diffusion line to low temperature can miss dominant boundary transport.

F

Fick’s first law
Fick’s first law relates local flux to the negative concentration gradient multiplied by diffusivity in the concentration-based model.
A concentration falling toward the right produces a positive rightward flux when diffusivity is positive.
Fick’s second law
Fick’s second law relates local concentration change with time to concentration-profile curvature when diffusivity is constant.
An upward-curving concentration profile indicates a positive local rate of concentration increase.
Fitted prefactor
A fitted prefactor is the Arrhenius multiplier recovered from diffusion measurements after the activation energy has been determined.
Substituting either of two measured coefficients into the fitted relation recovers the same prefactor before rounding.
Frenkel pair
A Frenkel pair consists of a vacancy and an interstitial ion formed when an ion moves from its normal site into a void.
A silver ion displaced into an interstitial site in AgCl leaves a vacancy at its original position.

G

Grain
A grain is an individual crystal within a polycrystalline solid, with a consistent lattice orientation through its interior.
Different grains in polished and etched brass can reflect light differently because their orientations differ.
Grain boundary
A grain boundary is a narrow bonded transition region joining two crystals with different lattice orientations in a polycrystal.
Preferential etching at grain boundaries produces the dark network visible in many optical micrographs.
Grain-boundary diffusion
Grain-boundary diffusion is transport along the less regularly packed regions between grains, usually faster than interior transport.
Refining the grains increases boundary area and can increase the importance of boundary transport.

H

Homologous temperature
Homologous temperature is absolute temperature divided by absolute melting temperature, used to compare thermal conditions across metals.
A temperature near 0.4 of the melting temperature can allow diffusion to matter over engineering times.

I

Interdiffusion
Interdiffusion is the migration of different elements into one another, producing a composition profile across the joined materials.
A heated copper–nickel diffusion couple develops a graded alloy region around its original interface.
Interstitial diffusion
Interstitial diffusion is movement of small atoms between neighboring spaces in the host lattice without requiring lattice vacancies.
Carbon usually moves much faster than host iron atoms because it travels between interstitial sites.
Interstitial solid solution
An interstitial solid solution contains small solute atoms in the spaces between the host crystal’s regular atomic sites.
Carbon dissolved in iron strains nearby atoms even though carbon is much smaller than an iron atom.
ISO grain size index
The ISO 643 grain size index for steel relates a logarithmic size number to grain count per square millimeter of specimen area.
An ISO index of 7 represents 1024 grains per square millimeter of the actual specimen.

J

Junction depth
Junction depth is the depth where introduced dopant concentration equals the concentration of the opposite-type background dopant.
The intersection of the dopant profile with the background level locates the modeled junction.

K

Kirkendall effect
The Kirkendall effect is displacement of lattice markers during interdiffusion caused by unequal opposing intrinsic atomic fluxes.
Markers on a brass core moved closer together when zinc left faster than copper entered during heating.

L

Lattice diffusion
Lattice diffusion is atomic transport through the regular crystal interior, using the appropriate vacancy or interstitial mechanism.
The large volume of grain interiors can outweigh their slower diffusivity in a coarse-grained hot metal.

M

Mass concentration
Mass concentration is the mass of a specified species per unit volume of the material, commonly expressed in kg/m³.
Using carbon concentration in kg/m³ gives a mass flux when Fick’s first law uses SI length and diffusivity.
Mean intercept length
Mean intercept length is the specimen test-line length divided by the number of grain-boundary intersections along that line.
Divide the image test-line length by magnification before using its boundary crossings to estimate grain size.
Microstructure
Microstructure is the size, shape and arrangement of structural features such as grains and phases that a microscope reveals.
Two pieces with the same overall composition can show different grain arrangements after different processing histories.
Mixed dislocation
A mixed dislocation has both edge and screw character because its local line direction is oblique to its Burgers vector.
A curved line can change from edge to screw character without changing its Burgers vector.

N

Nonsteady diffusion
Nonsteady diffusion is transport in which concentrations change with time because incoming and outgoing local fluxes do not balance.
Carbon concentration at a fixed depth rises during carburizing as the enriched region extends inward.

P

Phase boundary
A phase boundary is an interface between phases that differ in crystal structure, chemical composition or both.
A particle of a second phase embedded in a matrix is surrounded by an interface between the two phases.
Pre-exponential factor
The pre-exponential factor is the coefficient before the exponential in the Arrhenius relation and has the same units as diffusivity.
A prefactor tabulated in cm²/s must be multiplied by 10⁻⁴ before it is used with SI distances.
Predeposition
Predeposition is the doping stage in which an external supply maintains the silicon surface at a fixed dopant concentration.
A sustained dopant supply permits a constant-surface error-function profile to develop into silicon.

R

Reciprocal temperature
Reciprocal temperature is one divided by absolute temperature, expressed in inverse kelvins, and is the horizontal Arrhenius variable.
Moving to the right on a reciprocal-temperature plot means the material is at a lower temperature.
Resolution
Resolution is the smallest separation at which neighboring features can be distinguished as separate in a microscope image.
Increasing optical magnification cannot recover detail below the roughly 0.2 µm resolution limit.

S

Schottky pair
A Schottky pair in an AX ionic crystal consists of one cation vacancy and one anion vacancy that maintain charge neutrality.
In sodium chloride, removing one sodium ion and one chloride ion preserves the cation-to-anion ratio.
Screw dislocation
A screw dislocation is a line defect surrounded by a spiral arrangement of atomic planes, with its Burgers vector parallel to the line.
Following a plane around a screw dislocation resembles walking around a spiral ramp in the crystal.
Self-diffusion
Self-diffusion is the movement of atoms within a pure element without a change in its overall elemental concentration.
A tracer isotope can reveal copper atoms changing positions even when the copper composition stays uniform.
Self-interstitial
A self-interstitial is a host atom occupying a void between normal lattice sites, producing strong local distortion.
A host atom squeezed into a small void costs more formation energy than an empty lattice site.
Semi-infinite solid
A semi-infinite solid is a body whose far boundary remains effectively unaffected by diffusion during the treatment being modeled.
A thick steel part can retain its original composition far below the surface during a limited carburizing treatment.
Short-circuit path
A short-circuit path is a fast diffusion route along a surface, grain boundary or dislocation core through a less regular atomic arrangement.
At low temperature, fast paths may dominate and bend a polycrystal’s Arrhenius plot away from its lattice line.
Solid solution
A solid solution is a single solid phase in which solute atoms occupy sites within the solvent’s retained crystal structure.
Nickel can replace copper atoms while the Cu–Ni solution retains an FCC crystal structure.
Solubility limit
The solubility limit is the greatest amount of solute that can remain in a single solid solution under specified conditions.
Adding carbon beyond the amount stable in ferrite requires another phase to accommodate the excess.
Solute
A solute is a component dissolved in a larger amount of solvent, occupying regular lattice sites or interstitial spaces.
Carbon is an interstitial solute when it is dissolved between the regular atomic sites of iron.
Solvent
The solvent is the component present in the greatest amount in a solution and provides the host structure for dissolved atoms.
Copper is the solvent in alpha brass containing a smaller weight percentage of dissolved zinc.
Stacking fault
A stacking fault is an interruption in the normal sequence of atomic planes, such as a local change in close-packed stacking.
A short ABAB region in an otherwise ABCABC sequence gives a local HCP-like arrangement in an FCC metal.
Steady-state diffusion
Steady-state diffusion is transport with a concentration profile that remains unchanged in time because there is no local accumulation.
A plate can pass a continuous flow of hydrogen while each interior position keeps the same concentration.
Substitutional solid solution
A substitutional solid solution contains solute atoms on regular lattice sites that would otherwise hold host atoms.
The close atomic sizes of nickel and copper support extensive substitutional mixing in their FCC lattice.
Surface diffusion
Surface diffusion is movement of atoms along an external surface, often with a lower barrier than movement through the lattice.
A high surface diffusivity does not mean the surface route carries most of a thick specimen’s total mass.
Surface energy
Surface energy is the excess energy per unit area associated with atoms at a surface, where fewer neighboring bonds are present.
Reducing a liquid drop’s area lowers its total surface energy when its volume stays constant.

T

Tilt boundary
A small-angle tilt boundary is a boundary that can be represented as a wall of edge dislocations producing a small misorientation.
Increasing the dislocation spacing reduces the angle predicted by the small-angle tilt relation.
Twin boundary
A twin boundary is a special grain boundary across which the two crystal lattices have a specific mirror-image relationship.
Annealing twins commonly appear within FCC copper and brass after suitable heat treatment.

V

Vacancy
A vacancy is a normal lattice site with no atom in it, providing an empty destination for a neighboring lattice atom.
Heating aluminum sharply increases its equilibrium vacancy population and enables more atomic exchanges.
Vacancy diffusion
Vacancy diffusion is atomic movement by exchanges between atoms on normal lattice sites and neighboring empty lattice sites.
An iron atom entering an adjacent vacancy leaves a new vacancy behind at the site it formerly occupied.
Vacancy formation energy
Vacancy formation energy is the energy needed to create a vacancy, expressed per atom or per mole with matching constants.
An energy in eV per atom is combined with Boltzmann’s constant in eV/K in the exponential.
Volume defect
A volume defect is a three-dimensional imperfection such as a pore, crack or inclusion, usually much larger than atomic sites.
Shrinkage during casting can leave pores, while trapped slag creates foreign inclusions in steel.

W

Weight percent
Weight percent is an element’s mass divided by the total alloy mass, multiplied by 100; it is also called mass percent.
A 100 g sample of 30 wt% zinc brass contains 30 g of zinc and 70 g of the other component.

About this lesson

By StudeliReport a mistake

Make your own Study Materials

Turn your notes, slides and documents into Study Guides, Practice Questions, Flashcards and 6 more tools.

Get Started