Mechanical Properties of Materials

Learn how engineers measure how materials respond to load. Turn tensile and compression test readings into stress and strain, find the modulus of elasticity, yield strength and tensile strength from a stress–strain curve, and explain the difference between elastic and plastic deformation. Calculate ductility, resilience and toughness, compare the Rockwell, Brinell and Vickers hardness tests, and use the scatter in test results and a factor of safety to choose a working stress.

BeginnerLesson 4 of 9 in Materials Science and Engineering Course

What you will learn

  1. Explain how a tensile or compression test is run, turn its load and length readings into engineering stress and strain, and read the regions of a stress–strain curve for metals, ceramics and polymers.
    • Turn tensile test readings into engineering stress and strain
      Describe the tensile test, its specimen and measurements, and calculate engineering stress and strain from load and elongation readings.
    • Run compression, shear and torsion tests
      Explain when a compression, shear or torsion test is used, how compressive and shear stress and strain are defined, and how materials behave differently in compression.
    • Identify the regions of a stress–strain curve
      Read the elastic region, yielding, strain hardening, necking and fracture on an engineering stress–strain curve, and compare typical curves of metals, ceramics and polymers.
  2. Use Hooke's law, the modulus of elasticity, Poisson's ratio and the shear modulus to calculate elastic deformation, and explain why stiffness differs between materials.
    • Find the modulus of elasticity with Hooke's law
      Define elastic deformation, find the modulus of elasticity from the straight part of a stress–strain curve, and use Hooke's law to calculate elastic stress, strain and elongation.
    • Explain why stiffness differs between materials
      Relate the modulus of elasticity to atomic bonding, compare typical moduli of metals, ceramics and polymers, and describe nonlinear and time-dependent elastic behavior.
    • Use Poisson's ratio and the shear modulus
      Calculate lateral strain and changes in diameter with Poisson's ratio, and relate the shear modulus to the modulus of elasticity for isotropic materials.
  3. Explain what happens in a material when it deforms permanently, find the yield strength and tensile strength from a test, and describe necking, strain hardening, true stress and elastic recovery.
    • Find the yield strength and explain why metals deform permanently
      Describe plastic deformation at the atomic scale, find the yield strength with the 0.2 percent offset method, and recognize a yield point.
    • Determine tensile strength and describe necking and strain hardening
      Calculate tensile strength and fracture strength from test data, explain strain hardening and necking, and convert engineering values to true stress and true strain.
    • Predict elastic recovery after plastic deformation
      Calculate the permanent strain left after unloading from the plastic region, and explain springback and the higher yield strength on reloading.
  4. Calculate ductility as percent elongation and percent reduction in area, and calculate the elastic and total energy a material absorbs per unit volume as resilience and toughness.
    • Calculate and compare ductility
      Define ductility, calculate percent elongation and percent reduction in area from a broken specimen, and explain what the values mean for forming and safety.
    • Calculate resilience and toughness from the stress–strain curve
      Calculate the energy per unit volume a material stores elastically and absorbs up to fracture, and use these values to compare materials.
  5. Explain how the main hardness tests work, calculate and report hardness values on the right scale, and use hardness to estimate strength and check materials.
    • Compare the main hardness tests and scales
      Describe the Rockwell, Brinell, Vickers and Knoop indentation tests, their indenters, loads and notation, and the conditions for a valid result.
    • Calculate hardness and estimate strength from it
      Calculate Brinell and Vickers hardness from dent measurements, estimate tensile strength from hardness, and use conversion tables with their limits.
  6. Describe the scatter in measured material properties with an average and a standard deviation, and choose a working stress with a safety factor.
    • Describe the scatter in measured properties
      Explain why repeated tests on the same material give different results, and summarize test results with the average and the standard deviation.
    • Choose a working stress with a safety factor
      Calculate a working stress from the yield strength and a safety factor, size a simple tension rod with it, and explain how the safety factor is chosen.

Mechanical Properties of Materials study guide

6 chapters

1

Read tensile and compression test results

A testing machine first reports loads and movements. The material properties emerge when those readings are related to the specimen's dimensions and plotted as stress against strain. Follow the measurements through tension, compression and twisting, then compare the curve shapes of metals, ceramics and polymers. Specimen geometry and test conditions explain why a fair comparison needs more than two maximum-load readings.

1.1 From load and extension to stress and strain

A tensile test pulls a specimen along its axis while recording force and extension. Thick ends fit into the grips; the narrower, uniform middle carries the measurements and usually breaks away from the grips. Round specimens and flat dog-bone strips serve the same purpose. A slow, controlled pulling rate makes it possible to follow the response from initial loading to fracture.

Measure the right length and area

The gauge length, l0, is the marked length in the reduced section. An extensometer measures its change, Δl=l−l0. Crosshead movement also includes stretching of the machine and grips, so it can overstate the extension of the gauge length, especially during small elastic strains.

Engineering stress divides the force by the original cross-sectional area. Engineering strain divides extension by the original gauge length:

σ=FA0,ε=Δll0.

Stress measures load intensity; strain measures relative length change. Strain has no unit because the length units cancel. A strain of 0.002 means an extension of 0.2 percent, not 2 percent. Engineering stress keeps the original area in its denominator throughout the test, even when the specimen becomes thinner.

Work through a tensile reading

A round steel specimen starts with a diameter of 12.5 mm and a gauge length of 50.0 mm. At 30.0 kN, its measured extension is 0.059 mm.

  1. Use half the diameter as the radius: A0=π(6.25)2=122.7 mm2.
  2. Convert the force to newtons: 30.0 kN=30 000 N.
  3. Calculate stress: σ=30 000/122.718≈244.5 MPa.
  4. Calculate strain: ε=0.059/50.0=0.00118=0.118%.

The area was carried without rounding in the stress calculation. Using the diameter as the radius would make the area four times too large and the stress four times too small.

Compare results fairly

A force in newtons divided by an area in square millimeters gives MPa directly: 1 MPa=1 N/mm2. Moduli use GPa, with 1000 MPa in 1 GPa. For a data sheet in customary units, 1 ksi=1000 psi=6.895 MPa. Thus 244.5 MPa is about 35.5 ksi, and a modulus of 30 million psi is about 207 GPa.

Normalizing by area and gauge length removes the direct size effect during uniform deformation. Matching materials tested under matching conditions can then be compared through their curves. After necking, elongation also depends on specimen proportions and gauge length.

ASTM E8/E8M and ISO 6892-1 specify procedures for comparable tests. Most round E8 specimens use a gauge length of four diameters; E8M uses five. The usual ISO proportional length, 5.65S0, is about five diameters for a round section. Record the gauge length when reporting elongation at fracture.

Key Takeaways

  • Engineering stress uses original area; engineering strain uses original gauge length.
  • Measure gauge extension with an extensometer; crosshead travel includes machine movement.
  • N divided by mm² gives MPa; 0.002 strain is 0.2 percent.
  • Use the radius in the circular-area formula.
  • Gauge length matters when comparing elongation at fracture.

1.2 Compression and shear measurements

A compression test squeezes a short specimen between flat plates. Its original area and height provide the reference dimensions. The engineering formulas are the same as in tension, but shortening gives negative strain and compressive stress is negative. A report may instead give positive magnitudes labeled as compression; check the convention before combining values.

Why compression needs its own test

Concrete, stone and ceramic parts often carry compressive loads. Brittle materials are much stronger in compression than in tension because compression closes small cracks instead of pulling them open. Concrete's tensile strength is roughly one tenth of its compressive strength. A tensile result therefore cannot stand in for a compression result for these materials.

Consider a concrete cylinder 150 mm in diameter and 300 mm high that fails at 530 kN. Its original area is A0=π(75)2≈17 671 mm2. The failure stress has magnitude 530 000/17 671≈30.0 MPa. Under the signed convention, the compressive failure stress is −30.0 MPa.

A ductile metal usually shortens and widens without forming a tensile neck. Friction at the plates restrains its ends, making the middle bulge outward; this shape is barreling. A long, slender specimen may bend sideways through buckling, so the test would measure a structural instability instead of uniform compression. Short specimens reduce that problem. Standard concrete cylinders commonly have height twice their diameter. Many wrought metals have similar tensile and compressive yield strengths.

Shear changes angles

A force parallel to a surface produces shear stress, τ=F/A0. Shear deformation changes the angle between lines that were perpendicular. For a simple shear displacement, γ=tan⁡θ, where the small angular change is θ. At small angles, the angle in radians is nearly equal to its tangent. Degrees cannot be inserted directly into this small-angle relation.

In linear elastic shear,

τ=Gγ,

where G is the shear modulus. For steel with a shear modulus of 83 GPa under 50 MPa, first express the modulus as 83,000 MPa. Then γ=50/83 000≈6.0×10−4. This is a small angle of about 0.00060 rad. Dividing by 83 without converting units would overstate the strain a thousandfold.

Twisting produces shear

A torsion test twists a bar or tube and records torque and angle of twist. These readings, together with the specimen geometry, reveal its shear modulus and shear strength. The loading suits materials used in shafts, axles and drill bits. Torque is the turning action applied to the specimen; it is not itself a shear stress. The conversion from torque to stress depends on the cross-section, just as conversion from axial force to normal stress needs an area.

Key Takeaways

  • Compression uses negative stress and strain, or clearly labeled magnitudes.
  • Brittle materials resist compression much better than tension.
  • Plate friction causes barreling; slender specimens can buckle.
  • Elastic shear follows τ = Gγ, with small angles in radians.

1.3 What a stress–strain curve reveals

A stress–strain curve puts engineering stress on the vertical axis and engineering strain on the horizontal axis. Each feature answers a different question: how much elastic deformation occurs, when permanent deformation becomes significant, how large a load the specimen carries, and how much deformation occurs before fracture.

Follow a ductile metal through the test

The initial, steep straight region is elastic. Its slope measures stiffness. As yielding develops, permanent strain appears. The curve then rises through strain hardening: further plastic deformation requires increasing stress. The highest engineering stress is the tensile strength. Beyond that maximum, a narrow neck forms and the engineering curve descends until fracture.

Before necking, the gauge section extends approximately uniformly. After necking, most further extension concentrates in the neck. Engineering stress drops because the force drops while its original-area denominator stays fixed. The material in the neck can continue to strain harden as its area shrinks. The falling engineering curve alone therefore cannot identify the local material response.

Imagine a curve that first bends near 280 MPa, reaches a maximum of 460 MPa, and ends at 340 MPa. The 460 MPa peak is the tensile strength. The last value is the engineering fracture stress. A repeatable yield strength needs a defined yield criterion, such as the offset method, when the change from elastic to plastic behavior is gradual.

Compare material classes
Material behaviorTypical curveWhat to read
Ductile metalSteep start and a long plastic regionYield, peak, necking and fracture
Brittle glass or ceramicNearly straight to fractureStiffness and fracture strength; little plastic strain
Ductile polymerLower slope, yielding and extensive stretchingA neck can spread along the specimen
ElastomerStrongly curved, mostly recoverable extensionElastic behavior need not be linear

Annealed copper, aluminum and low-carbon steel can stretch substantially before breaking. Glass, most ceramics and gray cast iron usually break after little plastic deformation. Polystyrene and acrylic can be brittle at room temperature; polyethylene and nylon can show yielding and neck propagation. Rubbers can stretch several times their original length and still recover much of that extension.

Keep the test conditions with the curve

For most metals, increasing temperature lowers modulus, yield strength and tensile strength while increasing elongation. Polymers are particularly sensitive to temperature and pulling rate. A change of a few tens of degrees, or a faster test, can change the observed ductile or brittle behavior. Compare curves at matching test conditions before assigning their differences to composition.

A steep slope is evidence of high stiffness; it says little by itself about the height of the peak. The strain at fracture describes stretch to failure. The entire area under the curve measures energy absorbed per unit volume. Reading only the highest point misses these separate properties.

Key Takeaways

  • Read stiffness from the initial slope and tensile strength from the peak.
  • Yielding, strain hardening, necking and fracture are different stages.
  • After necking, engineering stress and local material stress tell different stories.
  • Brittle materials have little plastic strain; elastic rubbers can have curved responses.
  • Temperature and pulling rate affect the measured curve.
2

Explain and calculate elastic deformation

Small elastic movements determine how much a loaded part changes shape before permanent deformation begins. Connect the straight-line stress–strain slope to atomic bonding, calculate extension and lateral contraction, and see how Young's modulus links to shear modulus. Curved or delayed recoverable responses also matter, especially for polymers, so identifying the response regime comes before choosing an elastic equation.

2.1 Calculate elastic stiffness and extension

Elastic deformation disappears when the load is removed. Atoms move slightly from their equilibrium positions while keeping their neighbors, then return on unloading. Elastic strains in metals and ceramics are usually small, often below one percent. A specimen may therefore carry substantial stress while its extension is barely visible.

Use the straight part of the curve

For linear elastic behavior, Hooke's law is

σ=Eε.

The constant E is Young's modulus, or modulus of elasticity. It is the stress–strain slope and has stress units, usually GPa. A higher modulus means a smaller elastic strain under the same stress.

Find the slope from two points safely inside the straight region:

E=σ2−σ1ε2−ε1.

Use strain as a decimal. If the axis gives percentages, convert before calculating. Using a stress divided by its strain is appropriate when the straight line passes through the origin. Two interior points help avoid a small seating offset at the start of a real test.

Find a modulus from a reading

A steel specimen has stress 244.5 MPa at strain 0.00118 while still on its straight elastic line. Dividing gives about 207,000 MPa, or 207 GPa. If 0.118 were used in place of 0.00118, the inferred modulus would be a hundred times too small.

Predict extension in two steps

An aluminum alloy has E=69 GPa. A 300 mm bar carries 100 MPa elastically. Express both stresses in MPa, then find strain:

ε=100/69 000≈0.001449.

Multiply this dimensionless value by the original length:

Δl=εl0=(100/69 000)(300)≈0.435 mm.

The bar returns to its original length on unloading. Strain and extension are different quantities: doubling the original length at the same stress doubles extension but leaves strain unchanged.

Keep stiffness separate from strength
PropertyMeaningFeature of the curve
ModulusResistance to elastic strainInitial slope
Yield strengthStress associated with permanent deformationYield criterion or yield point
Tensile strengthMaximum engineering stressHighest point

A high-strength steel and a soft low-carbon steel have nearly the same modulus. Heat treatment can change their yield strengths greatly without making their elastic slopes much different. At equal stress, steel with a modulus near 207 GPa strains about one third as much as aluminum near 69 GPa. At equal force, cross-sectional area also affects the stress, so geometry must be included before comparing actual extensions.

Hooke's linear equation applies within the straight elastic region. Once significant plastic deformation occurs, total strain includes a permanent part. Dividing stress by modulus then gives only the recoverable elastic contribution, not the total strain.

Key Takeaways

  • Young’s modulus is the slope of the linear elastic curve.
  • Use decimal strain and matching stress units when finding E.
  • Find elastic extension from strain times original length.
  • Stiffness and strength measure different behavior.

2.2 Bond stiffness and curved elastic responses

Elastic stiffness begins with atomic bonds. At the equilibrium spacing, the net force between neighboring atoms is zero. Pulling them slightly apart produces a restoring force. The steeper the force–separation curve near equilibrium, the greater the force needed for a small displacement, and the higher the material's modulus.

Compare typical moduli

Strong bonding often accompanies a high melting point and a high modulus. The approximate values below show the scale of these differences.

MaterialApproximate Young's modulus
Tungsten407 GPa
Steel or nickel207 GPa
Copper110 GPa
Titanium107 GPa
Aluminum69 GPa
Magnesium45 GPa
Alumina380 GPa
Silica glass70 GPa
Many rigid plastics1–4 GPa

Ceramics often have high moduli because of strong ionic and covalent bonds, but the silica-glass value shows why a material class is not one fixed stiffness. Polymer chains can rotate, uncoil and move relative to one another. Weak secondary interactions between chains allow much larger deformation than small bond stretching alone. Rubbers can have moduli of only a few MPa.

Temperature affects these responses. As temperature rises, most materials become less stiff. Metals show a moderate reduction over ordinary temperature ranges. Polymers can lose stiffness sharply near the glass transition, where chain motion becomes much easier.

Changing strength does little to bond stiffness

Small changes in alloying, grain size or cold work can strongly change how easily dislocations move. They usually change atomic bond stiffness much less. Consequently, soft and hardened steels both have a modulus near 200 GPa. To reduce a part's elastic extension, a different material or a larger cross-section can be more effective than a different heat treatment.

Describe an elastic curve that is not straight

Elastic means recoverable, not necessarily proportional to stress. Gray cast iron, concrete and many polymers can have curved elastic responses. Two useful slope measures are:

  • Tangent modulus: the local slope at a chosen point, found with a tangent to the curve.
  • Secant modulus: the slope of the line from the origin to that point.

At a point with 20 MPa stress and 0.010 strain, the secant modulus is 20/0.010=2000 MPa=2.0 GPa. That one point does not give the tangent slope; nearby curve data are needed. State the stress level when reporting either modulus for a nonlinear response.

Some recoverable deformation takes time. Anelasticity describes delayed elastic strain or recovery. It is usually small in metals but much more noticeable in polymers, whose viscoelastic behavior combines elastic and time-dependent response. A polymer may keep stretching under a constant load, and recovery after unloading can also be delayed. A reading taken immediately and one taken after a hold can therefore differ.

Key Takeaways

  • Bond-force slope near equilibrium helps determine modulus.
  • Moduli vary widely within and between material classes.
  • Heat treatment changes steel strength much more than its modulus.
  • Tangent and secant moduli describe different slopes on a curved response.
  • Recoverable deformation can be nonlinear or delayed.

2.3 Lateral contraction and elastic constants

Stretching a bar makes it longer and slightly thinner. The strain along the load is axial strain; strains across the load are lateral strains. Taking tension as positive makes axial strain positive and lateral contraction negative. In compression, the signs reverse: the bar gets shorter and wider.

Poisson's ratio relates these small elastic strains:

ν=−εxεz,εx=−νεz.

The minus sign gives a positive ratio for ordinary materials that contract sideways in tension. Most metals lie near 0.25–0.35: steel about 0.30, aluminum about 0.33 and copper about 0.34.

Predict a diameter change

A steel rod starts at 10 mm diameter, with E=207 GPa and ν=0.30. Under an elastic tensile stress of 200 MPa:

  1. Axial strain is εz=200/207 000≈0.000966.
  2. Lateral strain is εx=−0.30(200/207 000)≈−0.000290.
  3. Diameter change is Δd=εxd0≈−0.00290 mm.

Apply lateral strain to diameter, not gauge length. The small decrease is consistent with elastic deformation; it is not the large local thinning of a plastic neck.

Work backward from a measurement

An aluminum rod of diameter 12 mm becomes 0.0020 mm thinner. Its modulus is 69 GPa and its Poisson's ratio is 0.33. The lateral strain is −0.0020/12=−0.0001667. Divide its magnitude by 0.33 to find axial strain, about 0.000505. Hooke's law then gives σ=69 000(0.00050505)≈34.8 MPa. Multiplying by π(6)2 gives a tensile force near 3940 N.

Connect Young's and shear moduli

An isotropic material has the same properties in every direction. Its linear elastic constants obey

E=2G(1+ν).

For aluminum, G=69/[2(1+0.33)]≈25.9 GPa. For ordinary metals, the shear modulus is roughly 0.4 times Young's modulus. Single crystals, wood and many composites are anisotropic; their properties depend on direction, so this isotropic relation cannot supply all of their elastic behavior.

For small uniaxial elastic strains, fractional volume change is εz(1−2ν). A ratio approaching 0.5, as in rubber, means almost no volume change. For steel at 0.30, elastic tension increases volume slightly. The limiting value 0.5 represents incompressibility in isotropic elasticity.

Use the elastic ratio only in its proper regime. During uniform plastic flow of a dense isotropic metal, volume is nearly constant. Each lateral plastic true-strain increment is then about −0.5 times the axial increment; finite engineering strains do not follow that same simple ratio.

Key Takeaways

  • Poisson’s ratio links lateral and axial elastic strains with opposite signs.
  • Multiply lateral strain by the original diameter to find diameter change.
  • E = 2G(1 + ν) applies to isotropic linear elasticity.
  • A Poisson’s ratio near 0.5 means nearly constant elastic volume.
  • Plastic lateral strain needs a plastic-flow description, not the elastic ratio.
3

Determine yield and tensile strength and explain plastic deformation

Permanent deformation changes both a specimen's shape and its later response to loading. Use a repeatable yield criterion to locate its onset, distinguish the maximum engineering stress from the stress at fracture, and track how a shrinking section changes the meaning of stress. Separating recovered strain from residual strain then explains reloading and the partial opening of a formed sheet after its load is removed.

3.1 Permanent deformation and the yield criterion

Plastic deformation remains after unloading. In a crystalline metal, dislocations move along crystal planes, allowing atoms to slip past one another in small steps. Bonds break and form with new neighbors along the moving dislocation. Moving this line defect takes much less stress than sliding an entire perfect atomic plane at once.

Materials differ in how easily they accommodate permanent change. Dislocations move with difficulty in many ionic and covalent ceramics, so these materials usually break with little plastic strain at room temperature. Polymer chains can slide and untangle; glass can flow permanently at high temperature.

Locate a repeatable yield value

The proportional limit marks departure from the straight stress–strain line. The elastic limit is the highest stress followed by complete recovery. These are different definitions, and both can be hard to locate precisely in a gradual transition. A standardized yield criterion gives a reproducible strength value for comparison and design.

The 0.2 percent offset method constructs a line with the original elastic slope but shifted right by a strain of 0.002. Its intersection with the measured curve gives the offset yield strength, written σy or Rp0.2. If unloading follows the elastic slope, the intersection leaves 0.002 permanent strain.

  1. Read the strain axis carefully: 0.2 percent is 0.002 in decimal form.
  2. Start the offset line at that strain on the horizontal axis.
  3. Keep it parallel to the initial elastic line.
  4. Read the stress where it intersects the test curve.

Starting at the origin would reproduce the elastic line and remove the specified offset. Rotating the line to meet a convenient data point would change the criterion.

Calculate an intersection

An aluminum alloy has E=70 GPa. Its offset line, in MPa, is σ=70 000(ε−0.002). Near the intersection, measured points are (0.0060, 300 MPa) and (0.0065, 310 MPa). Their segment slope is 10/0.0005=20 000 MPa.

Write the local test curve as σ=300+20 000(ε−0.0060). Equating it with the offset line gives 50 000ε=320, so ε=0.0064. The stress is 70 000(0.0064−0.002)=308 MPa. Total strain at that point is 0.0064; only 0.002 is permanent after elastic recovery.

Recognize a yield point

Some low-carbon steels show an upper yield point, then a drop to a lower yield level while deformation bands spread. Strain hardening follows the plateau. The lower yield level is commonly used as the yield strength. ISO symbols distinguish upper ReH from lower ReL yield strength.

Yield strength ranges from a few tens of MPa in soft pure aluminum to well above 1000 MPa in hardened steels. It is central to designs that must avoid permanent change of shape.

Key Takeaways

  • Plastic slip changes atomic neighbors through dislocation motion.
  • Proportional limit, elastic limit and offset yield are distinct definitions.
  • The 0.2 percent offset line starts at 0.002 strain and has slope E.
  • Read offset yield at the intersection, not at the strain-axis offset.
  • A yield-point steel has separate upper and lower yield levels.

3.2 Maximum load, necking and true values

Tensile strength, also called ultimate tensile strength, is the maximum engineering stress: TS=Fmax⁡/A0. Its ISO symbol is Rm. A specimen with original area 122.7 mm² and maximum load 55.2 kN has tensile strength about 450 MPa. This peak can occur long after yielding.

Why the curve rises, then falls

Plastic deformation multiplies dislocations and makes their motion harder as they obstruct one another. This strain hardening raises the stress required for further plastic flow. At the engineering-stress maximum, hardening can no longer compensate for shrinking cross-sectional area. Deformation localizes in a neck, the load falls, and fracture follows. Many ductile metals develop a cup-and-cone fracture there.

Engineering fracture stress uses the force at break and the original area. If that specimen breaks at 44.0 kN, its engineering fracture stress is about 359 MPa, below its 450 MPa maximum. For a brittle specimen that breaks at the peak, tensile strength and engineering fracture strength coincide.

Follow the changing dimensions

True stress uses the instantaneous area, σT=F/Ai. True strain accumulates incremental stretches and, for uniform axial extension, is εT=ln⁡(li/l0). For uniform plastic deformation with nearly constant volume:

σT=σ(1+ε),εT=ln⁡(1+ε).

At engineering stress 400 MPa and engineering strain 0.20, the true values are 480 MPa and about 0.182. The smaller current area raises true stress above engineering stress; logarithmic tensile strain is smaller than the corresponding engineering strain.

These global conversions stop working when a neck makes deformation nonuniform. After necking, measure the local neck area to find F/Ai. In a typical strain-hardening metal, true stress can continue rising while engineering stress falls. Global gauge extension cannot describe the local strain in the neck.

Fit the hardening response

Many metals in uniform plastic flow can be represented by σT=KεTn, where K is a strength coefficient and n is the strain-hardening exponent. Using two points:

n=ln⁡(σT2/σT1)ln⁡(εT2/εT1).

The points (0.10, 575 MPa) and (0.15, 617.7 MPa) give n≈0.177. Substitution gives K=575/0.100.176668≈864 MPa.

For this power-law model, necking begins when true strain reaches n. The predicted engineering strain is e0.176668−1≈0.193, or about 19 percent. Both fitting points lie before this predicted onset. A larger exponent, often around 0.1–0.5 for common metals, supports more uniform stretching before localization, which is useful in deep drawing.

Key Takeaways

  • Tensile strength is maximum force divided by original area.
  • Strain hardening comes from dislocations obstructing further motion.
  • Necking begins when hardening cannot offset area loss.
  • True stress uses current area; global conversions require uniform deformation.
  • For the power-law hardening model, true strain at necking equals n.
  • Engineering fracture stress can be lower than tensile strength.

3.3 Elastic recovery and permanent strain

Loading beyond yield produces two kinds of strain at once: elastic strain that can recover and plastic strain that remains. On unloading a typical metal, the stress–strain path is approximately straight and parallel to the original elastic line. The modulus controls the unloading slope even though the loading curve has entered the plastic region.

Separate the strain components

At the unloading point, read both stress and total strain. The recovered elastic strain is εe=σ/E. Subtract it from total strain to find permanent strain:

εp=ε−σE.

The subtraction is necessary because total strain was measured under load. Treating all of it as permanent overstates the residual extension. Treating unloading as a return along the original loading curve would wrongly erase the plastic strain.

For a steel with E=200 GPa loaded to 500 MPa at total strain 0.0100:

  1. Convert the modulus: 200 GPa is 200,000 MPa.
  2. Find elastic recovery: 500/200 000=0.0025.
  3. Find permanent strain: 0.0100−0.0025=0.0075.
  4. For a 50 mm gauge length, permanent extension is 0.0075(50)=0.375 mm.

The loaded extension was 0.500 mm. Removing 0.125 mm of elastic extension leaves the fitted-back length at 50.375 mm. This length check confirms the strain calculation without mixing percentages and decimals.

Reload a strain-hardened specimen

On reloading in the same direction, the specimen first follows approximately the unloading line upward. Plastic flow resumes near the previous unloading stress, now above the original yield strength. The metal was strengthened by its prior plastic deformation; it was not given a much larger elastic modulus.

Deliberate plastic deformation at room temperature is called cold work. Rolling, drawing and bending can use it to raise strength. It also uses up some ability to deform further before fracture, so ductility decreases. A steep unloading slope alone cannot tell how much cold work the specimen has received; the residual strain and renewed yield level carry that information.

Explain springback during forming

A sheet bent beyond yield opens slightly when the forming load is removed. This springback comes from recovery of the elastic part of its deformation. The permanent part keeps most of the new shape. At a given unloading stress, a lower modulus gives more recovery; a higher yield strength allows more elastic strain to build before plastic flow begins. High-strength, low-modulus materials therefore tend to show greater springback.

Forming tools often bend a sheet farther than the desired final angle to allow for this opening. The required allowance depends on the material's unloading response and forming conditions. Raising the force after plastic flow has begun does not make elastic recovery disappear; the unloading point still contains an elastic contribution.

Key Takeaways

  • Recovered strain equals unloading stress divided by modulus.
  • Subtract recovery from total strain to find permanent strain.
  • Same-direction reloading yields near the earlier unloading stress.
  • Cold work raises strength and reduces remaining ductility.
  • Springback is elastic recovery after forming.
4

Measure ductility and toughness

A strength value alone cannot describe how far a material can deform or how much energy it can absorb. Measurements on a broken specimen reveal permanent stretching and local thinning, while areas on the stress–strain curve reveal elastic storage and energy absorbed to fracture. Compare these measures with care: gauge length affects elongation, and the portion of curve included determines which energy property is being measured.

4.1 Ductility from a broken specimen

Ductility measures how much plastic deformation a material can undergo before fracture. A ductile metal can stretch or bend substantially, supporting forming operations and giving visible deformation before failure. A brittle material fractures with little plastic change. An elongation below about 5 percent is a useful rough description of brittle behavior, not a universal boundary between material classes.

Measure permanent length change

After the test, fit the broken pieces together and measure their final gauge length, lf. Elastic strain has recovered at fracture, so this measurement gives permanent extension. Percent elongation is

%EL=lf−l0l0×100.

The ISO symbol for this measure is A. A specimen with original gauge length 50.0 mm and fitted-back length 62.5 mm has %EL=(62.5−50.0)/50.0×100=25%. Its permanent extension is 12.5 mm. Using the loaded length just before fracture would include an elastic contribution.

Measure the local neck

Percent reduction in area compares the original area with the smallest area at the break:

%RA=A0−AfA0×100.

Its ISO symbol is Z. For a round specimen, area scales with diameter squared, giving

%RA=[1−(dfd0)2]×100.

If the original diameter is 12.5 mm and the final neck diameter is 7.9 mm, the remaining area fraction is (7.9/12.5)2=0.399424. The reduction is about 60.1 percent. Calculating only the percentage diameter decrease would give 36.8 percent, a different quantity.

Compare tests on the same basis

Elongation and reduction in area need not have similar numbers. Elongation averages permanent stretching over a gauge length. Reduction in area describes a highly local change at the neck. A specimen can therefore show 25 percent elongation and about 60 percent area reduction in the same test.

The neck contributes a concentrated extension. On a shorter gauge length, that contribution occupies a larger fraction of the measured length, raising percent elongation. Report a result as, for example, “25 percent in 50 mm.” Comparing it directly with a result measured over 100 mm can mistake a geometry effect for a material difference. Reduction in area does not use gauge length, although test conditions and material state still matter.

Ductility affects how far a sheet can bend, a wire can be drawn or a billet can be rolled before cracking. It also helps a loaded material change shape and redistribute load before fracture. Most metals become more ductile as temperature rises and less ductile after cold work. A high tensile strength by itself does not tell whether a material has enough ductility for a forming operation.

Key Takeaways

  • Percent elongation uses the fitted-back gauge length after fracture.
  • Percent area reduction uses the smallest area at the neck.
  • For round sections, square the diameter ratio.
  • Report gauge length with elongation; the two ductility measures are distinct.

4.2 Energy stored elastically and absorbed to fracture

Stress–strain area measures energy per unit volume. Multiplying stress by dimensionless strain gives units of J/m³. Numerically, an area in MPa corresponds directly to MJ/m³. The horizontal axis must use decimal strain: using a percentage-axis number without dividing by 100 overstates the energy a hundredfold.

Calculate resilience

Resilience is the capacity to store energy elastically and return it on unloading. The modulus of resilience, Ur, is the area under the elastic curve up to yield. A straight elastic region forms a triangle:

Ur=12σyεy=σy22E.

A spring steel with yield strength 1000 MPa and modulus 200 GPa has Ur=10002/(2×200 000)=2.5 MJ/m3. A steel yielding at 250 MPa with the same modulus stores only 2502/(2×200 000)=0.15625 MJ/m3. Quadrupling yield strength increases this elastic energy capacity sixteenfold because the strength is squared.

A good spring needs high yield strength so that substantial energy can be stored without permanent set. High stiffness alone is not enough: at fixed yield strength, a higher modulus reduces yield strain and the elastic triangle's area.

Calculate tensile toughness

Tensile toughness is the whole area under a slowly measured, unnotched tensile curve up to fracture. It includes the elastic and plastic portions. A material needs both useful stress capacity and substantial strain capacity to enclose a large area.

For a ductile metal, a rough rectangle estimate uses an average stress:

UT≈σy+TS2εf.

For yield strength 350 MPa, tensile strength 500 MPa and fracture strain 0.30, the average is 425 MPa. The estimated area is 425(0.30)=127.5 MJ/m3, or about 128 MJ/m³. This is an estimate; integrating measured data captures the actual curved shape and the post-peak segment.

For a brittle material with a straight curve right up to fracture, use the elastic triangle:

UT=σf22E.

Alumina at fracture stress 300 MPa and modulus 380 GPa has fracture strain about 0.000789. Its area is 3002/(2×380 000)≈0.118 MJ/m3. A similar order of strength therefore need not mean similar absorbed energy.

Read the property the application needs

The highest curve is not necessarily the one with the largest area. A very strong but brittle material can absorb less energy before fracture than a weaker, ductile metal. Hardness also gives no direct measure of this area. State the test type with a toughness value: tensile toughness in MJ/m³ differs from quantities obtained using notched or impact specimens.

Key Takeaways

  • Stress–strain area in MPa gives energy density in MJ/m³.
  • Resilience is the elastic area up to yield.
  • For linear elasticity, Ur = σy²/(2E).
  • Tensile toughness is total area to fracture and needs both strength and ductility.
  • A brittle straight-to-fracture curve has a triangular area.
  • Use decimal strain when calculating areas.
5

Measure and interpret hardness

A small indentation can provide a quick check on a material or a heat treatment. The result depends on the indenter, applied force and measured dent geometry, so a hardness number needs its scale and test conditions. Compare the common methods, calculate Brinell and Vickers results, and judge when an empirical hardness–strength estimate or a conversion table can support a useful comparison.

5.1 Choose and report a hardness test

Hardness is resistance to localized plastic deformation. Indentation tests press a hard tip into a prepared surface and measure the permanent dent's size or depth. At a fixed test condition, a smaller dent means a harder material. These quick tests leave a small mark and are useful for checking batches, heat treatments and finished parts.

The Mohs scale ranks mineral scratch resistance from 1 for talc to 10 for diamond. Engineering metals are more often tested with controlled indenters and forces.

Compare indentation methods
MethodIndenter and measurementUseful application
RockwellCone or ball; residual depth changeFast direct readings on production parts
BrinellTungsten carbide ball; dent diameterAveraging coarse-grained castings
VickersSquare diamond pyramid; two diagonalsWide hardness range and small regions
KnoopElongated diamond pyramid; long diagonalShallow testing of thin or brittle regions

A Rockwell minor load seats the indenter and establishes a depth reference. The added load is applied and removed, then the depth change is read under the minor load. Regular HRC uses a diamond cone and 150 kgf total force, about 1471 N. HRB uses a 1.588 mm ball and 100 kgf total, about 981 N. Both use a 10 kgf minor force, about 98 N. The total includes the minor force.

For regular scales, HR=N−h/(0.002 mm), where h is residual depth increase. The constant is 100 for diamond scales and 130 for ball scales. A C-scale increase of 0.076 mm gives 100−0.076/0.002=62, reported as “62 HRC.” Superficial scales use a 3 kgf minor force and total forces of 15, 30 or 45 kgf for thinner regions.

Brinell commonly uses a 10 mm ball and a load up to 3000 kgf. A result such as “229 HBW 10/3000” identifies the tungsten carbide ball, its diameter and force convention. The large dent samples a wider region than a microhardness impression.

Vickers uses a 136° square-based diamond pyramid. Measure both diagonals and use their mean. “618 HV 30” identifies a 30 kgf test. Small-force Vickers and Knoop tests can assess individual phases or thin hardened layers. Knoop's long, shallow impression particularly suits thin layers and brittle materials.

Prepare a valid measurement

Use a clean, smooth, flat surface and sufficient specimen thickness. A dent must not be influenced by the support beneath the specimen or by a nearby edge or impression. About ten indentation depths is a useful thickness guide for some methods; spacing of several dent widths is also needed. The exact thickness and spacing limits follow the chosen method, indenter and standard.

Always include the scale. Equal numbers on HRC and HRB are not equal hardness. Select a scale with a valid working range; readings below about 20 HRC call for a more suitable scale, often HRB for softer metals.

Key Takeaways

  • Hardness measures resistance to a local permanent dent or scratch.
  • Rockwell reads depth; Brinell reads dent diameter.
  • Vickers uses the mean of two diagonals; Knoop makes a shallow elongated dent.
  • Report the scale and test conditions with the number.
  • Thickness, surface quality and indentation spacing affect validity.

5.2 Calculate indentation hardness and estimate strength

A hardness calculation connects test force with indentation geometry. Check whether the equation expects newtons or kilograms-force before inserting the force. The hardness designation retains its scale and test conditions; it is not reported as an ordinary stress value in MPa.

Calculate Brinell hardness

With force F in kgf and ball diameter D and mean dent diameter d in mm:

HB=2FπD(D−D2−d2).

This uses the curved surface of the spherical impression. For a 10 mm ball, 3000 kgf force and 4.00 mm dent:

  1. Calculate 102−42=84≈9.16515.
  2. The denominator is π(10)(10−84)≈26.2275 mm2.
  3. Divide 6000/26.2275≈228.8.

Report “229 HBW 10/3000.” The dent is 0.40 times the ball diameter, within the usual range of about 0.24–0.60. With newtons, multiply the kgf-form equation's numerator by about 0.102 to preserve the hardness number. Using a dent radius in place of diameter changes the geometry incorrectly.

Calculate Vickers hardness

For Vickers, first average the two measured diagonals. With this mean d in mm:

HV=1.8544F/d2with F in kgf,

or HV=0.1891F/d2with F in N.

A 30 kgf force, about 294.2 N, and a mean diagonal of 0.300 mm give HV=1.8544(30)/(0.300)2≈618. The result is “618 HV 30.” Taking just the smaller diagonal would overstate hardness because diagonal length is squared in the denominator.

Use hardness to estimate strength

For many steels, tensile strength in MPa is approximately TS≈3.45HB. A Brinell value near 229 suggests a tensile strength near 3.45(229)=790 MPa. In customary units, the approximate steel relation is tensile strength in psi equal to 500 times HB. These are empirical correlations, with scatter, not exact identities. Brass, cast iron and other alloy groups require different relationships.

An estimate can help check a heat treatment or screen a batch. When a decision depends on a required minimum tensile strength, use tensile tests or the material specification. Hardness alone does not establish an exact strength.

Convert scales with material-specific data

ASTM E140 and ISO 18265 provide approximate conversions between indentation scales for particular material groups. Use the relevant group and range; a steel table cannot be applied to aluminum simply because both are metals. Direct testing on the required scale gives a firmer result.

Keep the properties distinct: hardness concerns local plastic deformation, modulus concerns elastic strain, and tensile toughness concerns energy absorbed to fracture. Hardening steel usually raises hardness and strength, changes modulus little, and reduces ductility.

Key Takeaways

  • Use the force unit required by the chosen hardness equation.
  • Brinell uses dent diameter and a spherical surface area.
  • Vickers uses the squared mean of two diagonals.
  • For many steels, TS in MPa is approximately 3.45 times HB.
  • Conversions depend on material group and are approximate.
  • Hardness, elastic stiffness and toughness are separate properties.
6

Allow for property variability with safety factors

Test results vary, and a service load is rarely known with perfect certainty. Summarize repeated measurements with a mean and sample standard deviation, then connect specified minimum strength to a working stress. A simple tension-rod calculation shows how that stress determines area and diameter. The final choice must account for rounding, uncertainty and the failure condition the calculation actually addresses.

6.1 Summarize scatter in test results

Repeated tests on the same named material do not produce one exact number. Composition and microstructure vary within and between batches. Specimen preparation, dimension measurements, machine calibration, pulling rate, temperature and setup can also change the result. A useful report describes both the center of the measurements and their scatter.

Calculate the sample mean and spread

For n measurements, the arithmetic mean is

xˉ=∑xin.

The sample standard deviation is

s=∑(xi−xˉ)2n−1.

Subtract the mean from each reading, square each deviation, add the squares, divide by one less than the number of readings, and take the square root. Squaring prevents positive and negative deviations from canceling. The final square root returns the spread to the original unit, such as MPa.

Four tensile strengths are 520, 512, 515 and 522 MPa. Their sum is 2069 MPa, so the mean is 517.25 MPa. The deviations are 2.75, −5.25, −2.25 and 4.75 MPa. Their squares add to 7.5625+27.5625+5.0625+22.5625=62.75 MPa2. Divide by 3 and take the square root to obtain s≈4.57 MPa.

A suitably rounded report is “517 ± 5 MPa, four tests,” with the ± quantity identified as one sample standard deviation. This spread is not the uncertainty of a guaranteed lower limit. Dividing by 4 would calculate the population-form spread of these four values, not the sample estimate used here.

Interpret a distribution

For a normal distribution, about 68 percent of values lie within one standard deviation of the mean and about 95 percent within two. The lower point xˉ−2s is exceeded by about 97.5 percent of that distribution because only one tail lies below it. Subtracting two standard deviations does not create an absolute minimum.

For example, a normal population centered at 500 MPa with standard deviation 20 MPa has its lower two-standard-deviation point at 460 MPa. Some values still fall below it. In a symmetric distribution, about half lie below the mean, so the mean is a poor choice for a minimum strength requirement.

Use specified minimum properties

A material specification states acceptance requirements, such as a minimum yield strength. These requirements provide a common basis for accepted batches. Designers normally start from the specified minimum, then apply the required safety factor. A small set of high test values does not raise that specified value.

Reducing measurement error and controlling manufacturing can reduce scatter, but the two sources are different. Recalibrating the machine addresses measurement bias; it cannot remove real differences in composition or heat treatment. Keep test conditions and the number of specimens in the report so that another reader can interpret the spread.

Key Takeaways

  • Report a center, a spread and the number of tests.
  • Sample standard deviation uses n − 1 and has the measurement’s units.
  • Normal-distribution percentages describe proportions, not guaranteed bounds.
  • Specified minimum strength provides a design basis below typical mean values.

6.2 Choose a working stress and a rod size

A material's measured strength is not usually the stress chosen for routine service. Loads and properties have uncertainty, and permanent deformation can already make a ductile part unusable. A factor of safety, N>1, reduces the strength to a working stress, also called an allowable stress.

For a ductile material designed against yielding:

σw=σyN.

Use the specified minimum yield strength when it is the material's design basis. For brittle materials with no useful yield point, use an appropriate fracture strength and usually a larger factor because failure gives little warning and strength scatter can be greater.

Size a simple tension rod

A steel rod must carry 50.0 kN. Its yield strength is 310 MPa and its factor of safety is 2.0.

  1. Working stress: σw=310/2.0=155 MPa.
  2. Required area: A≥50 000/155≈322.58 mm2.
  3. Required round diameter: d≥4A/π≈20.27 mm.

A reported minimum of 20.3 mm rounds this calculation for communication. Select an available diameter at least as large as the unrounded minimum. Choosing 20 mm gives an area of about 314.16 mm² and a stress of about 159.2 MPa, above the 155 MPa limit. Rounding down is therefore a change in the design, not harmless arithmetic.

An equivalent load-side approach

Instead of reducing the strength, increase the calculated stress by a design factor:

σd=N′σc.

Then require yield strength at least as large as this design stress. With equal factors, checking σc≤σy/N and checking Nσc≤σy are algebraically equivalent. Applying the same allowance to both sides would introduce an extra factor. Use the convention required by the design method.

Select a factor for the uncertainty

Factors for ductile metals often fall around 1.2–4 in introductory examples. Greater uncertainty in loads, properties or analysis calls for a greater allowance. Serious consequences of failure and brittle behavior also favor a larger factor. Better-known loads and properties can support smaller factors when weight or cost is important. Codes and design standards may prescribe factors for a particular application; a textbook range cannot replace those requirements.

The calculation addresses yielding under the stated tensile load. Other service conditions can set different limits. A slender compressed member can buckle, repeated loading can cause fatigue, and high temperature or corrosion can change performance. Those conditions need checks suited to their own failure modes; increasing a yield-based factor alone does not calculate them.

Key Takeaways

  • Working stress for a ductile material is yield strength divided by safety factor.
  • Required area is load divided by working stress.
  • Choose a diameter at least as large as the calculated minimum.
  • Reducing strength and factoring load are equivalent when used consistently.
  • Uncertainty, failure consequences and prescribed standards influence the factor.

Mechanical Properties of Materials examples

6 Walkthroughs

1

Read a test from the first measurement to fracture

13 steps
Convert test readings, distinguish loading modes, and explain what the engineering curve shows.
  1. 1
    IntroductionWhat the machine tells you

    A testing machine records force and movement. To describe the material, connect those readings to the specimen’s original area and marked gauge length.

    Follow a tensile specimen through those conversions, then compare compression and shear. The curve will reveal several properties, each taken from a different feature.

  2. 2
    ExplanationChoose the reference dimensions

    The grips hold the thick specimen ends; the reduced middle contains the gauge length. An extensometer measures extension within that marked length.

    Use the original cross-sectional area for engineering stress and original gauge length for engineering strain. Crosshead travel can include stretching outside the gauge section, especially important when the elastic extension is very small.

  3. 3
    ExampleConvert force to engineering stress

    A round specimen has diameter 12.5 mm. Its area is A0=π(6.25)2≈122.7 mm2. At 30.0 kN, convert the force to 30,000 N and divide by the unrounded area: σ≈244.5 MPa. The radius is half the diameter. Using 12.5 mm as the radius would make the area four times too large and the calculated stress four times too small.

  4. 4
    ExampleConvert extension to strain

    The same specimen has a 50.0 mm gauge length and extends by 0.059 mm. Engineering strain is ε=0.059/50.0=0.00118. Multiply by 100 to express it as 0.118 percent. Strain has no unit because both lengths use millimeters. A longer specimen at the same uniform strain would have more extension; equal strain does not mean equal extension in millimeters.

  5. 5
    ChallengeCheck the measurement choice

    Two identical specimens carry the same force. One strain is calculated from an extensometer and the other from larger crosshead movement. Which calculation gives a lower apparent modulus, and why?

    ---reveal---

    The crosshead calculation does. Equal original areas give equal stress, but the larger movement gives a larger apparent gauge strain. Dividing stress by that strain lowers the apparent modulus because machine and grip movement has been included.

  6. 6
    ExampleRead compression with its sign

    A cylinder of diameter 150 mm fails at a compressive load of 530 kN. Its original area is π(75)2≈17 671 mm2. The strength magnitude is 530 000/17 671≈30.0 MPa. Under the signed convention, stress is negative and shortening also gives negative strain. A report using positive magnitudes must identify them as compression.

  7. 7
    Key InsightDistinguish a bulge from sideways bending

    A ductile cylinder can spread without breaking in compression. Friction restrains its ends, so its middle bulges: barreling.

    A slender specimen may instead bend sideways through buckling. Keeping a compression specimen short helps measure its material response instead of that instability. Brittle materials benefit from compression because the loading closes small cracks instead of opening them.

  8. 8
    ConnectionTwisting reveals shear behavior

    Shear changes angles. For small elastic distortion, τ=Gγ. At 50 MPa and shear modulus 83 GPa, γ=50/83 000≈0.00060. The angular measure is in radians. A torsion test applies torque and measures twist; specimen geometry connects those readings to shear stress and strain. A shaft transmitting a turning force is therefore a shear application.

  9. 9
    ChallengeChoose a useful comparison

    A ceramic survives a large compressive stress but breaks at a much smaller tensile stress. Is that consistent with its brittle behavior? Explain the role of small cracks.

    ---reveal---

    Yes. Tension opens small cracks, while compression pushes them closed. A brittle material can therefore have very different strengths in the two loading modes. A tensile strength cannot simply be used as its compressive strength.

  10. 10
    ExplanationLocate the stages of a ductile curve

    Read the curve from left to right: a steep elastic region, yielding, rising stress through strain hardening, the tensile-strength maximum, necking, and fracture.

    The early slope measures stiffness. The peak measures maximum load per original area. During necking the load can fall even as the shrinking local region continues to harden, because engineering stress keeps using the original area.

  11. 11
    ExplanationCompare the material responses

    Glass and most ceramics usually show little plastic strain before fracture. Ductile metals have a long plastic region. Polymers can be brittle, yield and draw through a spreading neck, or recover large nonlinear strains as elastomers.

    Temperature and pulling rate matter strongly for polymers. A curve is a response under its test conditions, so compare matching conditions before assigning a difference to composition.

  12. 12
    ChallengeRead several features together

    Two curves have equal initial slopes. P reaches a higher peak but breaks at very small strain; Q has a lower peak and a broad plastic region. What can you conclude about stiffness, tensile strength and toughness?

    ---reveal---

    Their initial stiffnesses match, and P has higher tensile strength. Toughness depends on total area under the curve, so the peak alone cannot decide it. The broad plastic region may give Q more area, but the actual areas are needed for the comparison.

  13. 13
    RecapKeep each curve feature tied to its property

    Use original dimensions for engineering quantities and measure the gauge section directly. Compression and shear require their own loading descriptions.

    On a tensile curve, read stiffness from slope, yielding from the appropriate criterion, and tensile strength from the maximum. Deformation to fracture and curve area add information that none of those stress values supplies alone.

2

Calculate recoverable changes in length and diameter

14 steps
Find elastic slopes, connect stiffness to bonding, and use Poisson’s ratio and isotropic elastic constants.

Save this lesson to follow every Walkthrough step by step.

  1. 1
    IntroductionStart with recovery and the response shape
  2. 2
    ExampleFind the elastic slope
  3. 3
    ExampleFind strain before extension
  4. 4
    ExampleConvert that strain into millimeters
  5. 5
    ChallengeSeparate stiffness from strength
  6. 6
    AnalogyConnect slope to atomic bonds
  7. 7
    ExplanationGive a curved response a defined slope
  8. 8
    ConnectionAllow for delayed elastic response
  9. 9
    ChallengeCheck what a single point establishes
  10. 10
    ExampleFind lateral strain with its sign
  11. 11
    ExampleApply lateral strain to the diameter
  12. 12
    ExplanationLink elastic constants only for isotropy
  13. 13
    ChallengeInfer stress from a shrinking diameter
  14. 14
    RecapChoose the relation that matches the response
3

Track yielding, hardening and elastic recovery

16 steps
Find offset yield, follow changing dimensions, and separate recovered strain from permanent deformation.

Save this lesson to follow every Walkthrough step by step.

  1. 1
    IntroductionPermanent change affects the next loading too
  2. 2
    ExplanationSlip advances through moving dislocations
  3. 3
    ExplanationBuild the offset line
  4. 4
    ExampleDescribe the measured segment
  5. 5
    ExampleFind where the two lines meet
  6. 6
    ChallengeCheck the meaning of the intersection
  7. 7
    ExampleUse maximum load for tensile strength
  8. 8
    Key InsightSeparate hardening from area loss
  9. 9
    ExampleConvert before necking
  10. 10
    ExampleFit the uniform hardening law
  11. 11
    ChallengePredict uniform extension before necking
  12. 12
    ExplanationRead the unloading slope
  13. 13
    ExampleFind the residual length
  14. 14
    ConnectionConnect reloading to cold work
  15. 15
    ChallengeExplain a formed sheet’s partial recovery
  16. 16
    RecapTrack the stress definition and the strain part
4

Measure plastic stretch and stress–strain area

11 steps
Calculate the two ductility measures, elastic energy storage and tensile toughness.

Save this lesson to follow every Walkthrough step by step.

  1. 1
    IntroductionLook beyond the peak stress
  2. 2
    ExampleFit the broken pieces together
  3. 3
    ExampleMeasure the neck’s area change
  4. 4
    Key InsightCheck what each percentage measures
  5. 5
    ChallengeCompare two gauge lengths
  6. 6
    ExplanationRead energy from an area
  7. 7
    ExampleCalculate the elastic triangle
  8. 8
    ExampleEstimate a ductile curve’s total area
  9. 9
    ChallengeCompare a narrow brittle curve
  10. 10
    ChallengeChoose the property for the task
  11. 11
    RecapKeep geometry and curve boundaries visible
5

Choose an indenter and calculate hardness

12 steps
Compare indentation methods, calculate results, and judge hardness-based strength estimates.

Save this lesson to follow every Walkthrough step by step.

  1. 1
    IntroductionA dent needs a test identity
  2. 2
    ExplanationRead Rockwell depth
  3. 3
    ExampleTurn depth into a scale number
  4. 4
    ExplanationChoose the optical method
  5. 5
    TipPrepare enough material around the dent
  6. 6
    ChallengeSelect the right local measurement
  7. 7
    ExampleSet up the Brinell geometry
  8. 8
    ExampleFinish and report Brinell hardness
  9. 9
    ExampleAverage Vickers diagonals first
  10. 10
    ConnectionUse a correlation for a suitable alloy group
  11. 11
    ChallengeDecide whether an estimate establishes a minimum
  12. 12
    RecapReport the test and respect the estimate
6

Turn variable test results into a working-stress check

12 steps
Calculate sample statistics, use a specified minimum, and select a passing tension-rod diameter.

Save this lesson to follow every Walkthrough step by step.

  1. 1
    IntroductionFrom test scatter to a service limit
  2. 2
    ExplanationSeparate material variation from measurement effects
  3. 3
    ExampleCalculate the sample center
  4. 4
    ExampleCalculate the sample standard deviation
  5. 5
    ExplanationRead the lower tail correctly
  6. 6
    ChallengeCompare a favorable mean with a requirement
  7. 7
    ExampleChoose the working stress
  8. 8
    ExampleFind the required area
  9. 9
    ExampleSelect a diameter that actually passes
  10. 10
    TipUse one factor convention consistently
  11. 11
    ChallengeCheck the strength basis and the size
  12. 12
    RecapState what the calculation checks

Mechanical Properties of Materials practice questions

50 Practice Questions in 5 sets

Set 1: Read measurements and identify properties10 Practice Questions

Question 1 of 10

A flat tensile specimen has an original area of 80 mm² and carries 16.0 kN. What is its engineering stress?
  1. 20.0 MPa
  2. 0.200 MPa
  3. 200 MPa
  4. 800 MPa
Show answerHide answer
Answer: C
Engineering stress is force divided by original area: 16,000 N divided by 80 mm² gives 200 MPa. A newton per square millimeter equals a megapascal. The value 0.200 comes from inserting 16 kN as though it were 16 N, leaving the force conversion undone.

Question 2 of 10

A tensile specimen has area 60 mm² and gauge length 40 mm. At 12 kN, a gauge extensometer reads 0.040 mm extension while the crosshead moves 0.080 mm. Both readings are in the linear range. What modulus and interpretation follow?
  1. 100 GPa; the gauge reading misses half the strain.
  2. 100 GPa; the crosshead is the gauge-length measurement.
  3. 200 GPa; the crosshead records only plastic extension.
  4. 200 GPa; the extra motion includes the machine and grips.
Show answerHide answer
Answer: D
The stress is 200 MPa and the gauge strain is 0.040/40 = 0.001, giving a modulus of 200 GPa. The crosshead includes motion outside the gauge section. Using its 0.080 mm as gauge extension would double the strain and halve the apparent modulus to 100 GPa.

Question 3 of 10

A short ductile cylinder develops a bulging middle during compression between unlubricated plates. What causes this shape?
  1. Friction restrains expansion near the ends.
  2. Buckling causes uniform sideways expansion.
  3. Uniform necking reduces the middle section.
  4. Elastic recovery expands the middle first.
Show answerHide answer
Answer: A
Plate friction holds back lateral expansion at the ends, while the middle can spread farther outward, producing barreling. Buckling instead bends a slender specimen sideways. Barreling describes a nonuniform bulge during compression, not the local loss of area called necking in tension.

Question 4 of 10

An elastic stress–strain line passes through (0.0004, 84 MPa) and (0.0014, 284 MPa). What Young’s modulus does its slope give?
  1. 203 GPa
  2. 200 GPa
  3. 210 GPa
  4. 284 GPa
Show answerHide answer
Answer: B
The stress change is 200 MPa and the strain change is 0.0010, so the slope is 200,000 MPa, or 200 GPa. Dividing 84 MPa by 0.0004 gives 210 GPa, but that uses an origin-to-point ratio. The two supplied points determine the slope even when the line has a small offset.

Question 5 of 10

A steel is hardened by heat treatment. Its yield strength rises greatly. What change in Young’s modulus is usually expected?
  1. It rises in proportion to yield strength.
  2. It remains approximately the same.
  3. It falls in proportion to ductility.
  4. It rises to the ceramic modulus range.
Show answerHide answer
Answer: B
Heat treatment changes the resistance to plastic deformation much more than the stiffness of atomic bonds. The steel’s elastic modulus therefore stays near its original value even when yield strength rises greatly. Assuming both properties rise together confuses the onset of permanent strain with the size of elastic strain.

Question 6 of 10

On a strain axis labeled in mm/mm, where does the line for a 0.2 percent offset yield construction start?
  1. At 0.002 strain and zero stress.
  2. At 0.2 strain and zero stress.
  3. At zero strain and 0.2 MPa stress.
  4. At 0.020 strain and zero stress.
Show answerHide answer
Answer: A
The offset is 0.2 divided by 100, or 0.002 strain, on the horizontal axis. From there the line runs parallel to the initial elastic slope until it meets the measured curve. Starting at 0.2 would represent a 20 percent strain offset, a hundred times the intended amount.

Question 7 of 10

A metal specimen begins to neck at a load of 28 kN and breaks at 23 kN. Its original area is 70 mm². What is its tensile strength?
  1. 329 MPa
  2. 400 MPa
  3. 70.0 MPa
  4. 500 MPa
Show answerHide answer
Answer: B
Tensile strength uses the maximum load and original area, so 28,000/70 gives 400 MPa. The 23 kN reading gives about 329 MPa, which is the engineering stress at fracture. A ductile specimen can break after its load has dropped below the earlier maximum during necking.

Question 8 of 10

A broken round specimen has an original diameter of 10 mm and a neck diameter of 8 mm. What is its percent reduction in area?
  1. 20 percent
  2. 64 percent
  3. 36 percent
  4. 80 percent
Show answerHide answer
Answer: C
The remaining area fraction is the squared diameter ratio, (8/10)² = 0.64. Subtracting from one gives a 36 percent area reduction. The 20 percent decrease describes diameter only; using it for area misses the square in the circular-area relationship.

Question 9 of 10

Which hardness test determines its result from a residual depth change under a preliminary load?
  1. Vickers
  2. Knoop
  3. Brinell
  4. Rockwell
Show answerHide answer
Answer: D
Rockwell measures the increase in indentation depth after the added load is removed, with the preliminary load still applied. Brinell measures dent diameter, while Vickers and Knoop use optical measurements of impression diagonals. Confusing a force application with an optical size measurement would select the wrong method.

Question 10 of 10

Two batches each have a mean yield strength of 420 MPa. Their sample standard deviations are 5 MPa and 18 MPa. What does the comparison show?
  1. The 5 MPa batch has less scatter around the same mean.
  2. The 18 MPa batch has a mean strength 13 MPa higher.
  3. The 5 MPa batch has no readings below 415 MPa.
  4. The 18 MPa batch has a guaranteed minimum of 402 MPa.
Show answerHide answer
Answer: A
A smaller standard deviation means results cluster more closely around the mean, so the 5 MPa batch has less measured scatter. Both means remain 420 MPa. Subtracting one standard deviation does not establish a guaranteed minimum; values can fall farther from the mean.
Set 2: Connect deformation, energy and hardness10 Practice Questions

Save this lesson to see every answer and practice every set.

Question 1 of 10

A 240 mm bar with modulus 120 GPa carries a tensile stress of 75 MPa within its linear elastic range. How far does it extend?
  1. 0.625 mm
  2. 1.50 mm
  3. 0.150 mm
  4. 0.0150 mm
Show answerHide answer

Save this lesson to see this answer.

Question 2 of 10

A 16 mm diameter rod has an elastic axial strain of 0.0015 and Poisson’s ratio 0.28. What is its diameter change?
  1. +0.00672 mm
  2. −0.0240 mm
  3. −0.00672 mm
  4. −0.0840 mm
Show answerHide answer

Save this lesson to see this answer.

Question 3 of 10

A metal’s engineering stress–strain curve reaches a maximum and then falls while a neck grows. Which property is read at the maximum?
  1. Yield strength
  2. Tensile strength
  3. Elastic limit
  4. Fracture strain
Show answerHide answer

Save this lesson to see this answer.

Question 4 of 10

An alloy has modulus 80 GPa. Near yield its measured curve is a straight segment from (0.0050, 280 MPa) to (0.0060, 300 MPa). What stress does the 0.2 percent offset construction give?
  1. 293 MPa
  2. 280 MPa
  3. 300 MPa
  4. 320 MPa
Show answerHide answer

Save this lesson to see this answer.

Question 5 of 10

A metal with modulus 150 GPa is unloaded from 450 MPa at total strain 0.0180. What permanent strain remains?
  1. 0.0030
  2. 0.0150
  3. 0.0210
  4. 0.0180
Show answerHide answer

Save this lesson to see this answer.

Question 6 of 10

A stress–strain area is calculated using stress in MPa and decimal strain. What energy-density unit has the same numerical value?
  1. kJ/m³
  2. J/mm³
  3. MJ/m³
  4. MJ/mm³
Show answerHide answer

Save this lesson to see this answer.

Question 7 of 10

Two linear elastic materials have the same yield strength. Material Q has twice the modulus of material P. How does Q’s modulus of resilience compare with P’s?
  1. It is half as large.
  2. It is four times as large.
  3. It is unchanged.
  4. It is twice as large.
Show answerHide answer

Save this lesson to see this answer.

Question 8 of 10

A Vickers test uses 20 kgf and gives a mean diagonal of 0.400 mm. What hardness should be reported, using HV = 1.8544F/d²?
  1. 92.7 HV 20
  2. 232 HV 20
  3. 37.1 HV 20
  4. 463 HV 20
Show answerHide answer

Save this lesson to see this answer.

Question 9 of 10

A round rod must carry 36 kN. Its specified minimum yield strength is 270 MPa and its safety factor is 2.5. Available diameters are 20, 21, 22 and 24 mm. What is the smallest acceptable size?
  1. 20 mm
  2. 21 mm
  3. 24 mm
  4. 22 mm
Show answerHide answer

Save this lesson to see this answer.

Question 10 of 10

A coarse-grained casting needs a hardness measurement that averages over a relatively large impression. Which method best fits that aim?
  1. Low-force Knoop
  2. Superficial Rockwell
  3. Low-force Vickers
  4. Brinell
Show answerHide answer

Save this lesson to see this answer.

Set 3: Interpret changing dimensions and test scatter10 Practice Questions

Save this lesson to see every answer and practice every set.

Question 1 of 10

A tensile specimen with a 60 mm gauge length extends by 0.090 mm. A second specimen of the same material has a 100 mm gauge length and reaches the same uniform engineering strain. What is its extension?
  1. 0.054 mm
  2. 0.250 mm
  3. 0.090 mm
  4. 0.150 mm
Show answerHide answer

Save this lesson to see this answer.

Question 2 of 10

A short compression specimen starts at 40 mm height and reaches 39.92 mm under a 24 kN compressive load. Its original area is 200 mm². What signed engineering stress and strain does it have?
  1. −120 MPa and +0.0020
  2. −120 MPa and −0.0002
  3. −120 MPa and −0.0020
  4. +120 MPa and −0.0020
Show answerHide answer

Save this lesson to see this answer.

Question 3 of 10

A nonlinear elastic curve passes through the origin and through 30 MPa at strain 0.015. What secant modulus corresponds to that point?
  1. 30 GPa
  2. 0.50 GPa
  3. 4.0 GPa
  4. 2.0 GPa
Show answerHide answer

Save this lesson to see this answer.

Question 4 of 10

An isotropic rod has modulus 90 GPa, Poisson’s ratio 0.25 and original diameter 20 mm. Under a linear elastic tensile load, its diameter falls by 0.004 mm. What axial stress does the measurement imply?
  1. 4.5 MPa
  2. 72 MPa
  3. 45 MPa
  4. 288 MPa
Show answerHide answer

Save this lesson to see this answer.

Question 5 of 10

A uniformly deforming metal has engineering stress 360 MPa and engineering strain 0.15 in a plastic, nearly constant-volume region. What are its true stress and true strain?
  1. 313 MPa and 0.140
  2. 414 MPa and 0.150
  3. 360 MPa and 0.163
  4. 414 MPa and 0.140
Show answerHide answer

Save this lesson to see this answer.

Question 6 of 10

A specimen starts with area 100 mm². At one reading it carries 40 kN with area 80 mm²; later, after necking, it carries 35 kN with neck area 50 mm². How do engineering stress and true stress at the neck change?
  1. They fall from 400 to 350 MPa and from 500 to 438 MPa.
  2. They fall from 400 to 350 MPa and rise from 500 to 700 MPa.
  3. They rise from 500 to 700 MPa and fall from 400 to 350 MPa.
  4. They rise from 400 to 700 MPa and remain at 500 MPa.
Show answerHide answer

Save this lesson to see this answer.

Question 7 of 10

Two identical long metal specimens develop the same localized neck extension. Elongation is reported over a 25 mm gauge length for one and 50 mm for the other. How does the neck’s contribution to percent elongation compare?
  1. It is larger for the 50 mm gauge.
  2. It is larger for the 25 mm gauge.
  3. It is the same for both gauges.
  4. It is determined only by final area.
Show answerHide answer

Save this lesson to see this answer.

Question 8 of 10

A steel has Vickers diagonals 0.390 and 0.410 mm under 196.14 N. Use HV = 0.1891F/d². What result follows, with the force designation expressed in kgf? Take 1 kgf = 9.807 N.
  1. 232 HV 20
  2. 232 HV 196
  3. 244 HV 20
  4. 221 HV 20
Show answerHide answer

Save this lesson to see this answer.

Question 9 of 10

Three yield-strength readings are 390, 400 and 410 MPa. What mean and sample standard deviation should be reported?
  1. 400 ± 8.2 MPa
  2. 400 ± 100 MPa
  3. 400 ± 10 MPa
  4. 400 ± 20 MPa
Show answerHide answer

Save this lesson to see this answer.

Question 10 of 10

A ductile material has specified minimum yield strength 480 MPa and a required safety factor of 3. What working stress follows?
  1. 160 MPa
  2. 1440 MPa
  3. 477 MPa
  4. 240 MPa
Show answerHide answer

Save this lesson to see this answer.

Set 4: Check methods and combine properties10 Practice Questions

Save this lesson to see every answer and practice every set.

Question 1 of 10

A torsion test gives a shear modulus of 30 GPa. At a small elastic shear strain of 0.0008, what shear stress corresponds to this response?
  1. 24 MPa
  2. 37.5 MPa
  3. 240 MPa
  4. 2.4 MPa
Show answerHide answer

Save this lesson to see this answer.

Question 2 of 10

A material shows large extension on a strongly curved loading path and returns to its original length when unloaded. How is this behavior classified?
  1. Strain hardening
  2. Linear plastic
  3. Linear elastic
  4. Nonlinear elastic
Show answerHide answer

Save this lesson to see this answer.

Question 3 of 10

Two rods have equal original lengths and areas. P has modulus 70 GPa and yield strength 350 MPa; Q has modulus 210 GPa and yield strength 250 MPa. At a tensile stress of 200 MPa, how do their strains and remaining yield-stress margins compare?
  1. Q strains one third as much; Q has the larger yield margin.
  2. Q strains one third as much; P has the larger yield margin.
  3. Q strains three times as much; P has the larger yield margin.
  4. Q strains three times as much; Q has the larger yield margin.
Show answerHide answer

Save this lesson to see this answer.

Question 4 of 10

A low-carbon steel curve rises to 325 MPa, drops to a 295 MPa yield plateau, then rises to a 440 MPa maximum. What lower yield strength and tensile strength should be reported?
  1. 295 MPa and 440 MPa
  2. 325 MPa and 295 MPa
  3. 295 MPa and 325 MPa
  4. 325 MPa and 440 MPa
Show answerHide answer

Save this lesson to see this answer.

Question 5 of 10

A 100 mm gauge length is loaded to 600 MPa at total strain 0.0120, then unloaded. The modulus is 200 GPa and unloading is linear. When the same specimen is reloaded to 300 MPa in the same direction, what gauge length is predicted before renewed plastic flow?
  1. 101.05 mm
  2. 100.90 mm
  3. 101.20 mm
  4. 100.15 mm
Show answerHide answer

Save this lesson to see this answer.

Question 6 of 10

Two materials have straight elastic regions. P yields at 600 MPa with modulus 100 GPa; Q yields at 900 MPa with modulus 225 GPa. What is their resilience comparison?
  1. P stores 2.25 times as much as Q.
  2. Q stores 1.5 times as much as P.
  3. Q stores 2.25 times as much as P.
  4. Both store 1.8 MJ/m³ before yield.
Show answerHide answer

Save this lesson to see this answer.

Question 7 of 10

A regular Rockwell C test gives a residual depth increase of 0.090 mm. What hardness does HR = 100 − h/0.002 give?
  1. 45 HRC
  2. 90 HRC
  3. 55 HRC
  4. 10 HRC
Show answerHide answer

Save this lesson to see this answer.

Question 8 of 10

A Brinell test uses a 5 mm carbide ball, 750 kgf and a 2.00 mm dent. Use HB = 2F/[πD(D − √(D² − d²))]. For this steel, estimate tensile strength in MPa as 3.45HB. What paired result follows?
  1. 945 HBW 5/750 and about 3260 MPa
  2. 57 HBW 5/750 and about 198 MPa
  3. 229 HBW 5/750 and about 229 MPa
  4. 229 HBW 5/750 and about 790 MPa
Show answerHide answer

Save this lesson to see this answer.

Question 9 of 10

A normally distributed strength population has mean 560 MPa and standard deviation 25 MPa. Approximately what fraction exceeds 510 MPa?
  1. 68 percent
  2. 95 percent
  3. 97.5 percent
  4. 50 percent
Show answerHide answer

Save this lesson to see this answer.

Question 10 of 10

Why is yield strength commonly used as the strength basis for a ductile part that must retain its shape?
  1. Yield strength is the maximum load divided by current area.
  2. Permanent deformation can make the part unusable before fracture.
  3. Elastic deformation becomes permanent at every stress level.
  4. Yield strength is the energy absorbed before the part fractures.
Show answerHide answer

Save this lesson to see this answer.

Set 5: Resolve competing interpretations10 Practice Questions

Save this lesson to see every answer and practice every set.

Question 1 of 10

The same polymer is tested at the same pulling rate at 15 °C and 55 °C. It is brittle in the colder test and ductile in the warmer test. How should the results be interpreted?
  1. The tests establish that modulus is unchanged by temperature.
  2. The warmer result replaces the colder result for all service conditions.
  3. Temperature changes the response, so both conditions must be reported.
  4. The cold specimen’s low elongation means it has greater toughness.
Show answerHide answer

Save this lesson to see this answer.

Question 2 of 10

On a curved elastic stress–strain response, which modulus is the slope of the tangent at a specified stress?
  1. Secant modulus
  2. Tangent modulus
  3. Shear modulus
  4. Strength coefficient
Show answerHide answer

Save this lesson to see this answer.

Question 3 of 10

An isotropic material has Young’s modulus 120 GPa and shear modulus 48 GPa. Under a small uniaxial elastic tensile strain of 0.0020, what lateral strain and fractional volume change are predicted?
  1. −0.0010 and 0
  2. −0.0005 and 0.0020
  3. +0.0005 and 0.0030
  4. −0.0005 and 0.0010
Show answerHide answer

Save this lesson to see this answer.

Question 4 of 10

Uniform plastic true-stress data follow σT = KεTⁿ through (0.04, 250 MPa) and (0.16, 500 MPa). What engineering strain is predicted at the onset of necking by this model?
  1. 0.500
  2. 0.160
  3. 0.649
  4. 0.250
Show answerHide answer

Save this lesson to see this answer.

Question 5 of 10

Two metals are unloaded from the same tensile stress after plastic deformation. P has half the modulus of Q, and both unload linearly. How does their recovered strain compare?
  1. P recovers half as much strain as Q.
  2. P recovers twice as much strain as Q.
  3. Both recover the same strain.
  4. Their recovery is fixed by total strain alone.
Show answerHide answer

Save this lesson to see this answer.

Question 6 of 10

A round specimen starts with gauge length 80 mm and diameter 12 mm. After fracture and fitting the pieces together, its gauge length is 96 mm and neck diameter is 9 mm. What elongation and area reduction should be reported?
  1. 16 percent and 25.0 percent
  2. 20 percent and 25.0 percent
  3. 16 percent and 43.8 percent
  4. 20 percent and 43.8 percent
Show answerHide answer

Save this lesson to see this answer.

Question 7 of 10

Approximate two slow tensile curves as straight lines joining the stated (decimal strain, MPa) points. P passes through (0, 0), (0.002, 400) and (0.10, 600), then fractures at (0.20, 300). Q passes through (0, 0) and fractures at (0.003, 700). What toughness comparison follows?
  1. P: 94.4 MJ/m³; Q: 1.05 MJ/m³.
  2. P: 120 MJ/m³; Q: 1.05 MJ/m³.
  3. P: 49.4 MJ/m³; Q: 1.05 MJ/m³.
  4. P: 94.4 MJ/m³; Q: 2.10 MJ/m³.
Show answerHide answer

Save this lesson to see this answer.

Question 8 of 10

A shallow hardness measurement is needed on a very thin brittle layer. Which indenter shape best suits this aim?
  1. An elongated Knoop diamond pyramid.
  2. A large spherical Brinell ball.
  3. A regular Rockwell B ball.
  4. A regular Rockwell C cone.
Show answerHide answer

Save this lesson to see this answer.

Question 9 of 10

A laboratory reports 240 HB for a steel and uses TS ≈ 3.45HB in MPa. A design requires a certified minimum tensile strength of 820 MPa. How should the report inform acceptance?
  1. It suggests about 69.6 MPa; reject using the inverse correlation.
  2. It proves 828 MPa; the part meets the 820 MPa requirement.
  3. It suggests about 828 MPa; the specified minimum still needs verification.
  4. It proves 820 MPa; round down the correlation to the requirement.
Show answerHide answer

Save this lesson to see this answer.

Question 10 of 10

A rod carries 42 kN. The batch mean yield strength is 360 MPa, but its specified minimum is 300 MPa. A safety factor of 2.4 is required and available diameters are 20, 21, 22 and 24 mm. What smallest diameter meets the yield-based working-stress check?
  1. 21 mm
  2. 22 mm
  3. 20 mm
  4. 24 mm
Show answerHide answer

Save this lesson to see this answer.

Stuck on your own question? Homework Help

Key Terms

79 Key Terms, each with its definition

A

Anelasticity
Anelasticity is recoverable deformation that develops or disappears gradually, so part of an elastic response occurs after a time delay.
A specimen with delayed elastic recovery continues returning toward its original shape after unloading.
Anisotropy
Anisotropy means a material's properties depend on direction, so one axial modulus cannot describe all possible loading orientations.
A single crystal or fiber composite can have different moduli along different directions.
Axial strain
Axial strain is the relative length change along a loading axis, positive for extension and negative for shortening under the usual convention.
A tensile rod's axial strain comes from its gauge extension divided by original gauge length.

B

Barreling
Barreling is the outward bulging of a compression specimen's middle when friction at the loading plates restrains sideways expansion at its ends.
A metal cylinder becomes wider at the center while its ends are held back by plate friction.
Brinell test
The Brinell test presses a carbide ball into a surface and uses the measured dent diameter and test force to determine hardness.
A large Brinell impression helps average local differences within a coarse-grained casting.
Brittleness
Brittleness is a tendency to fracture with little plastic deformation, giving limited permanent stretching or bending before the material breaks.
A glass tensile specimen usually breaks without the long plastic region typical of annealed copper.
Buckling
Buckling is sideways instability of a slender compressed specimen that prevents the test from representing uniform axial compression.
A long thin test piece can bend sideways before its material reaches compressive yield.

C

Cold work
Cold work is deliberate plastic deformation at room temperature, such as rolling or drawing, that raises strength while reducing remaining ductility.
A drawn wire can yield at a higher stress than the same metal before its plastic deformation.
Compression test
A compression test squeezes a specimen between loading plates to measure its behavior under shortening, including compressive strength or yield.
A short concrete cylinder is compressed to measure the load it can sustain before failure.

D

Design stress
Design stress is the calculated service stress multiplied by a design factor, giving the strength requirement in a load-side allowance method.
A calculated stress of 100 MPa with a design factor of 2.5 requires strength of at least 250 MPa.
Ductility
Ductility is the amount of plastic deformation a material can undergo before fracture and is commonly measured by elongation or area reduction.
A ductile metal can be drawn into wire without cracking as early as a brittle material would.

E

Elastic deformation
Elastic deformation is a reversible change in shape or dimensions that disappears when the applied load is removed and the material recovers.
A lightly loaded metal bar returns to its original length when its elastic tensile load is removed.
Elastic limit
The elastic limit is the highest stress after which a specimen fully recovers its original dimensions when the applied load is removed.
A loading–unloading test checks whether a small permanent extension remains after release.
Elastic recovery
Elastic recovery is the strain removed on unloading; for a linearly unloading metal it equals the unloading stress divided by Young's modulus.
At 400 MPa and modulus 200 GPa, the recovered elastic strain is 0.002.
Elastic region
The elastic region is the part of a loading response in which deformation can recover after unloading; its shape may be straight or curved.
A rubber specimen can show a curved elastic region while recovering a large extension.
Elastomer
An elastomer is a polymer capable of large, mostly recoverable strains with a nonlinear stress–strain response, as seen in many rubbers.
A rubber strip stretches several times its length and largely returns when released.
Energy density
Energy density is energy per unit volume; stress–strain area in MPa gives the same numerical value in MJ/m³ when strain is a decimal.
An elastic triangular area of 0.8 MPa represents stored energy density of 0.8 MJ/m³.
Engineering fracture stress
Engineering fracture stress is the force at the instant of fracture divided by the specimen's original cross-sectional area.
A ductile metal can have a fracture stress below its earlier maximum engineering stress.
Engineering strain
Engineering strain is the change in gauge length divided by the original gauge length, giving a dimensionless measure of relative extension.
An extension of 0.20 mm over 100 mm is an engineering strain of 0.002, not 0.20.
Engineering stress
Engineering stress is axial force divided by the original cross-sectional area, which remains the reference area as the specimen changes shape.
A force of 9000 N on an original area of 30 mm² gives engineering stress of 300 MPa.
Equilibrium spacing
The equilibrium spacing is the separation between neighboring atoms at which their net interaction force is zero before a small elastic displacement.
Elastic tension moves neighboring atoms slightly away from their equilibrium separation.
Extensometer
An extensometer measures the change in a selected specimen length directly, helping separate gauge extension from machine and grip movement.
Small elastic strains are measured on the gauge section with a clip-on extensometer.

F

Factor of safety
A factor of safety is a number greater than one used to provide a strength allowance for uncertainty in a stated design check.
Dividing a 360 MPa yield strength by a factor of 3 gives a 120 MPa working stress.
Fracture
Fracture is the breaking of a specimen, ending a tensile test after little plastic strain in brittle materials or much more in ductile ones.
A brittle glass specimen may reach its maximum tensile stress at the instant of fracture.

G

Gauge length
The gauge length is the original marked length of the specimen's reduced section over which extension is measured during a tensile test.
A 50 mm gauge length extending by 0.10 mm gives engineering strain 0.002, or 0.2 percent.
Glass transition
The glass transition is a temperature region where a polymer's chain mobility changes markedly and its mechanical stiffness can drop sharply.
A polymer part can become much less stiff when heated through its glass-transition region.

H

Hardness
Hardness is resistance to localized plastic deformation, measured by a controlled indentation or by resistance to scratching in a scratch test.
A smaller indentation under the same indenter and force indicates a harder test region.
Hardness conversion
A hardness conversion is an approximate correspondence between scales based on tests for a particular material group and applicable range.
A steel conversion table should not be used to assign an aluminum alloy a Rockwell value.
Hardness–strength correlation
A hardness–strength correlation is an empirical estimate linking indentation resistance and tensile strength for a specified material group.
For many steels, a Brinell hardness of 200 suggests tensile strength near 690 MPa.
Hooke's law
Hooke's law states that stress is proportional to strain in a linear elastic response, with Young's modulus as the proportionality constant.
Within the straight elastic range, doubling stress doubles the axial strain in a metal bar.

I

Incompressibility
Incompressibility means volume stays constant during deformation; isotropic linear elastic behavior approaches this limit as Poisson's ratio approaches 0.5.
Rubber's near-incompressible response balances axial stretching with sideways contraction.
Isotropy
Isotropy means a material has the same properties in every direction, allowing its linear elastic constants to be linked by a simple relation.
For isotropic elasticity, knowing Young's modulus and Poisson's ratio determines shear modulus.

K

Kilogram-force
A kilogram-force is a force unit equal to about 9.807 N, historically used to designate indentation loads and select hardness formula coefficients.
A Vickers force designated as 10 kgf corresponds to about 98.07 N in an SI calculation.
Knoop test
The Knoop test uses an elongated diamond pyramid that leaves a shallow impression suited to thin layers and brittle materials.
A thin ceramic layer can be sampled with a shallow Knoop impression and optical measurement.

L

Lateral strain
Lateral strain is the relative dimension change perpendicular to the loading axis, usually negative during tension of ordinary materials.
A shrinking rod diameter gives a negative lateral strain even while the axial strain is positive.

M

Mean diagonal
The mean diagonal in a Vickers test is the arithmetic average of the two indentation diagonals, used before squaring in the hardness equation.
Diagonals of 0.280 and 0.320 mm give a mean of 0.300 mm for the Vickers calculation.
Megapascal
A megapascal is one million pascals and equals one newton per square millimeter, making it a convenient stress unit for material tests.
Dividing a load in newtons by an area in square millimeters gives a stress directly in MPa.
Microhardness
Microhardness describes small-force indentation testing of tiny regions, such as individual phases, coatings or hardened surface layers.
A microhardness survey can compare the surface layer with the softer material beneath it.
Modulus of resilience
The modulus of resilience is elastic energy stored per unit volume up to yield, equal to the elastic area under the stress–strain curve.
For a linear response, squaring yield strength and dividing by twice the modulus gives this area.
Mohs scale
The Mohs scale ranks mineral scratch resistance from talc at 1 to diamond at 10 and differs from force-controlled metal indentation scales.
A mineral that scratches another has the higher scratch resistance in their Mohs comparison.

N

Necking
Necking is localized thinning during tension that begins when hardening can no longer compensate for area loss and maximum load is reached.
After necking starts, most additional extension occurs within the narrowed part of the specimen.
Normal distribution
A normal distribution is a symmetric bell-shaped distribution with about 68 percent of values within one standard deviation of its mean.
For a normal strength distribution, about 2.5 percent lie below the mean minus two standard deviations.

O

Offset yield strength
Offset yield strength is the stress where a line shifted by a specified strain and parallel to the elastic slope intersects the measured curve.
The 0.2 percent construction uses a line starting at decimal strain 0.002 on the strain axis.

P

Percent elongation
Percent elongation is the permanent increase in gauge length after fracture divided by original gauge length and multiplied by 100.
A 40 mm gauge length fitted back to 48 mm after fracture has 20 percent elongation.
Percent reduction in area
Percent reduction in area is the loss of cross-sectional area at the fracture neck divided by original area and multiplied by 100.
A section shrinking from 100 to 45 mm² has a 55 percent reduction in area.
Permanent strain
Permanent strain is the strain remaining after unloading, found by subtracting the recoverable elastic part from the total loaded strain.
A loaded strain of 0.015 with elastic recovery 0.003 leaves permanent strain of 0.012.
Plastic deformation
Plastic deformation is a lasting change in shape or dimensions that remains after unloading because the material's internal arrangement has changed.
A metal strip bent beyond yield keeps much of its new shape after the force is removed.
Poisson's ratio
Poisson's ratio is minus the lateral elastic strain divided by axial elastic strain in uniaxial loading, linking sideways and length changes.
A ratio of 0.30 gives lateral contraction equal to 30 percent of the small axial tensile strain.
Proportional limit
The proportional limit is the stress at which the initial straight stress–strain relationship ends, so stress is no longer proportional to strain.
A curve's first departure from a straight line marks the proportional limit, not its maximum stress.

R

Required area
The required area for a simple tension rod is load divided by working stress, providing the minimum section for that yield-based check.
A 20 kN load and 100 MPa working stress require at least 200 mm² of cross-sectional area.
Resilience
Resilience is the capacity to absorb energy through elastic deformation and return that energy as the material recovers on unloading.
A spring stores energy elastically during loading and gives it back when the force is removed.
Rockwell test
The Rockwell test measures hardness from the residual indentation-depth increase after an added load is removed while a minor load remains.
A regular HRC measurement uses a diamond cone and a total force designated as 150 kgf.

S

Sample mean
The sample mean is the sum of measured property values divided by the number of measurements, describing the center of the observed results.
A mean strength of 500 MPa can arise from a batch containing values both above and below it.
Sample standard deviation
The sample standard deviation measures scatter around the sample mean using squared deviations divided by n − 1, followed by a square root.
A 6 MPa sample standard deviation means less spread than 20 MPa around the same mean.
Secant modulus
The secant modulus is the slope from the origin to a selected point on a nonlinear response and must be reported with the point's stress level.
At 12 MPa and strain 0.006, the secant modulus is 2000 MPa, which is 2 GPa.
Shear modulus
The shear modulus is the ratio of shear stress to shear strain in a linear elastic response and measures resistance to angular distortion.
A material with a larger shear modulus has less elastic distortion under the same shear stress.
Shear strain
Shear strain measures angular distortion between initially perpendicular lines and is approximately the small angular change in radians.
A small shear strain of 0.001 corresponds to about 0.001 rad of angular distortion.
Shear stress
Shear stress is force parallel to a surface divided by the area carrying that force, describing the intensity of tangential loading.
A sliding force of 600 N over 20 mm² produces an average shear stress of 30 MPa.
Slip
Slip is plastic deformation in a crystal produced mainly by dislocations moving along crystal planes and leaving atoms with new neighbors.
Moving a dislocation lets a metal deform without sliding an entire perfect atomic plane at once.
Specified minimum strength
A specified minimum strength is a material acceptance requirement used as a design basis instead of assuming every part reaches the sample average.
A rod design uses the required 300 MPa minimum even if a few batch tests average 330 MPa.
Springback
Springback is partial recovery of a formed part's shape after unloading because its elastic deformation disappears while its plastic deformation remains.
A bent sheet opens slightly after release, so the forming tool may need to overbend it.
Stiffness
Material stiffness describes resistance to elastic strain and is characterized by an elastic modulus; a part's stiffness also depends on geometry.
Two rods of the same steel can extend differently under equal force if their areas differ.
Strain hardening
Strain hardening is the increase in resistance to plastic flow as prior deformation multiplies dislocations and makes their motion more difficult.
After yielding, a ductile metal can need increasing stress to keep deforming uniformly.
Strain-hardening exponent
The strain-hardening exponent is the power n in the uniform plastic-flow model σT = KεTⁿ and indicates the rate of hardening with true strain.
Within this power-law model, a larger n predicts more uniform stretching before necking.
Strength coefficient
The strength coefficient is the constant K in the power-law plastic-flow equation and has stress units when true strain is dimensionless.
After finding the exponent from two points, one point can be used to calculate K.
Stress–strain curve
A stress–strain curve plots stress against strain to show stiffness, yielding, strength and deformation capacity under specified test conditions.
The early slope and the later peak of a tensile curve describe different material properties.

T

Tangent modulus
The tangent modulus is the local slope at a specified point on a nonlinear stress–strain response, describing stiffness near that point.
A tangent drawn at the chosen stress gives a slope that can differ from the origin-to-point slope.
Tensile strength
Tensile strength is the maximum engineering stress reached in a tensile test, calculated as the highest force divided by the original area.
A peak load of 60 kN over an original 120 mm² section gives tensile strength of 500 MPa.
Tensile test
A tensile test pulls a specimen along its axis while recording force and gauge extension to measure its response through fracture.
A metal supplier uses a tensile test to report yield strength, tensile strength and elongation.
Tensile toughness
Tensile toughness is energy absorbed per unit volume through fracture in a slow, unnotched tensile test, equal to the entire stress–strain area.
A broad ductile-metal curve can absorb more energy than a higher but very narrow brittle curve.
Torsion test
A torsion test twists a bar or tube and records torque and twist angle, using specimen geometry to determine the material's shear response.
A torsion test helps characterize a metal intended for a shaft that transmits turning force.
True strain
True strain accumulates incremental relative stretches and equals the natural logarithm of current length divided by original length for uniform extension.
A uniform engineering strain of 0.25 corresponds to true strain ln(1.25), about 0.223.
True stress
True stress is instantaneous force divided by the current cross-sectional area, making dimensional changes part of the stress calculation.
A shrinking neck can raise true stress while falling load lowers the engineering stress.

U

Uniform elongation
Uniform elongation is extension distributed over the tensile gauge section before deformation concentrates in a local neck.
At the maximum load, uniform elongation ends and further extension concentrates in the neck.

V

Vickers test
The Vickers test uses a square-based diamond pyramid and calculates hardness from force and the mean of the impression's two diagonals.
A small-force Vickers test can compare individual phases in a polished metal sample.
Viscoelastic behavior
Viscoelastic behavior combines elastic response with time-dependent deformation, making loading duration and recovery time important in polymers.
A polymer can continue stretching under a held load and show delayed recovery after release.

W

Working stress
Working stress is the allowed service stress for the chosen strength basis and safety factor, such as yield strength divided by the factor.
A rod's calculated tensile stress must stay at or below the selected working stress.

Y

Yield point
A yield point is a distinct stress feature at the start of plastic flow, often with an upper peak followed by a lower plateau in low-carbon steel.
An initial stress drop can distinguish the upper yield point from the lower yield plateau.
Young's modulus
Young's modulus is the slope of the straight axial stress–strain response and measures how strongly a material resists elastic stretching.
Steel's modulus near 200 GPa is much larger than the modulus of a typical rigid plastic.

About this lesson

By StudeliReport a mistake

Make your own Study Materials

Turn your notes, slides and documents into Study Guides, Practice Questions, Flashcards and 6 more tools.

Get Started